How hard and how strong will a steel be after quenching and tempering at a given temperature? This tempering chart compares 30 oil quenched and 6 water quenched carbon and low alloy steels tempered at 205, 315, 425, 540 and 650°C, side by side. Every value is taken from our individual material data sheets, and every cell links to its source data sheet.
Use it to pick a grade and tempering temperature for a target hardness or tensile strength, or to see how much strength a grade keeps at higher tempering temperatures where toughness and ductility improve.
Tempering Chart: Hardness of Oil Quenched Steels by Tempering Temperature
Tempering Chart: Tensile Strength of Oil Quenched Steels by Tempering Temperature
Tempering Chart: Yield Strength of Oil Quenched Steels by Tempering Temperature
Tempering Chart: Water Quenched Steels
The data sheets below are for water quenching. Water quenching gives a faster cooling rate than oil, so compare these values only with each other or use them alongside the oil quenched tables with that in mind.
Hardness of Water Quenched Steels (HV)
Tensile Strength of Water Quenched Steels (MPa)
Which Steel and Tempering Temperature Reaches a Target Strength?
The table lists, for each minimum tensile strength target, the oil quenched grades whose data sheet minimum reaches the target, with the highest tempering temperature that still does so. A higher tempering temperature generally means better toughness and ductility at that strength.
| Minimum tensile strength | Oil quenched grades (highest tempering temperature reaching it) |
|---|---|
| ≥ 800 MPa | 1050 (425°C), 1060 (540°C), 1080 (650°C), 1095 (650°C), 1137 (315°C), 1141 (540°C), 1340 (540°C), 4037 (315°C), 4042 (540°C), 4140 (540°C), 4150 (650°C), 4340 (650°C), 5046 (540°C), 50B46 (650°C), 50B60 (650°C), 5130 (540°C), 5140 (540°C), 5150 (540°C), 5160 (650°C), 6150 (650°C), 81B45 (650°C), 8630 (540°C), 8640 (650°C), 86B45 (650°C), 8650 (650°C), 8740 (650°C), 9255 (650°C), 94B30 (540°C) |
| ≥ 1000 MPa | 1080 (540°C), 1095 (425°C), 1141 (425°C), 1340 (425°C), 4042 (425°C), 4140 (425°C), 4150 (540°C), 4340 (540°C), 5046 (425°C), 50B46 (425°C), 50B60 (540°C), 5130 (425°C), 5140 (425°C), 5150 (540°C), 5160 (540°C), 6150 (540°C), 81B45 (425°C), 8630 (425°C), 8640 (425°C), 86B45 (425°C), 8650 (540°C), 8740 (540°C), 9255 (540°C), 94B30 (425°C) |
| ≥ 1200 MPa | 1141 (315°C), 1340 (315°C), 4042 (315°C), 4140 (315°C), 4150 (425°C), 4340 (425°C), 5046 (315°C), 50B46 (425°C), 50B60 (425°C), 5130 (315°C), 5140 (315°C), 5150 (425°C), 5160 (425°C), 6150 (425°C), 81B45 (425°C), 8630 (315°C), 8640 (425°C), 86B45 (425°C), 8650 (425°C), 8740 (425°C), 9255 (425°C), 94B30 (425°C) |
| ≥ 1400 MPa | 1141 (205°C), 1340 (315°C), 4042 (315°C), 4140 (315°C), 4150 (315°C), 4340 (315°C), 5046 (205°C), 50B46 (315°C), 50B60 (315°C), 5130 (205°C), 5140 (315°C), 5150 (315°C), 5160 (425°C), 6150 (315°C), 81B45 (315°C), 8630 (205°C), 8640 (315°C), 86B45 (315°C), 8650 (315°C), 8740 (315°C), 9255 (425°C), 94B30 (315°C) |
| ≥ 1600 MPa | 1340 (205°C), 4042 (205°C), 4140 (205°C), 4150 (205°C), 50B46 (315°C), 50B60 (315°C), 5140 (205°C), 5150 (205°C), 5160 (315°C), 6150 (205°C), 81B45 (205°C), 86B45 (205°C), 8650 (205°C), 8740 (205°C), 9255 (315°C) |
Steel Tempering Chart FAQ
In our data sheets AISI 5160 is the hardest oil quenched grade tempered at 205°C, at 563–693 HV.
Oil quenched AISI 4140 drops from 455–565 HV at 205°C to 210–260 HV at 650°C, and tensile strength from 1600–1950 MPa to 680–840 MPa.
Oil quenched grades whose data sheet minimum tensile strength is 1400 MPa or more at 425°C or higher (highest such tempering temperature in brackets): 5160 (425°C), 9255 (425°C).
Tempering relieves the hard, brittle martensite formed during quenching. Higher tempering temperatures go further, lowering hardness and strength while improving ductility and toughness, as the tables above show for every grade.
Only with care. Water cools faster than oil, so water quenched data sheets show higher hardness for the same grade and tempering temperature. That is why this chart lists them in separate tables.
Related comparisons: AISI 4130 vs 4140 | AISI 4140 vs 4340 | low alloy steel grades | medium and high carbon steel grades
Need quenched and tempered steel parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.


One Reply to “Steel Tempering Chart: Hardness and Tensile Strength of Carbon and Alloy Steels at 205–650°C”
Comments are closed.