AISI 5140 Oil Quenched & Tempered at 540°C Material Data Sheet

AISI 5140 Oil Quenched & Tempered at 540°C Material Data Sheet

AISI 5140 Oil Quenched & Tempered at 540°C Overview

AISI 5140 tempered 540°C is AISI 5140 low alloy steel (UNS G51400, EN 41Cr4) in the oil quenched & tempered at 540°C condition. This AISI 5140 tempered 540°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 5140 conditions in our AISI 5140 yield, tensile and hardness comparison. Looking for AISI 5140 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5140 steel parts in-house and inspects them before shipment.

AISI 5140 Oil Quenched & Tempered at 540°C Designation

AISI 5140
ConditionTempered at 540°C & oil quenched
UNS numberG51400
US nameSAE 5140, ASTM 5140, ASTM 5140H, ASTM 5140, ~ASTM G51400
EN name~41CrS4, ~41Cr4
EN number~1.7045, ~1.7039, ~1.7035
ISO name~ 41 CrS 4, ~ 41 Cr 4, ~41Cr4
GB (Chinese) name~ 40Cr, ~40Cr, ~38CrA
JIS (Japanese) name~SCr440M

AISI 5140 Oil Quenched & Tempered at 540°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 5140 Oil Quenched & Tempered at 540°C Composition detail

C (carbon)0.38–0.43%
Cr (chromium)0.7–0.9%
Fe (iron)97.3–98.1%
Mn (manganese)0.7–0.9%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 5140 Oil Quenched & Tempered at 540°C Physical properties

Density7.8–7.9g/cm3

AISI 5140 Oil Quenched & Tempered at 540°C Mechanical properties

Young’s modulus209–217GPa
Specific stiffness26.6–27.7MN.m/kg
Yield strength (elastic limit)770–955MPa
Tensile strength900–1100MPa
Specific strength98.1–122kN.m/kg
Elongation13–21% strain
Compressive strength770–955MPa
Flexural modulus209–217GPa
Flexural strength (modulus of rupture)770–955MPa
Shear modulus80–85GPa
Bulk modulus162–177GPa
Poisson’s ratio0.285–0.295 
Shape factor29
Hardness – Vickers255–315HV
Elastic stored energy (springs)1410–2120kJ/m3
Fatigue strength at 10^7 cycles397–458MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
347–524MPa

AISI 5140 Oil Quenched & Tempered at 540°C Impact & fracture properties

Fracture toughness44–75MPa.m0.5
Toughness (G)9.62–25kJ/m2

AISI 5140 Oil Quenched & Tempered at 540°C Thermal properties

Melting point1430–1510°C
Maximum service temperature500–530°C
Minimum service temperature-68–-38°C
Thermal conductivity44–49W/m.°C
Specific heat capacity430–480J/kg.°C
Thermal expansion coefficient12–13.5µstrain/°C
Thermal shock resistance280–358°C
Thermal distortion resistance3.37–3.95MW/m
Latent heat of fusion265–280kJ/kg

AISI 5140 Oil Quenched & Tempered at 540°C Electrical properties

Electrical resistivity20–26µohm.cm
Electrical conductivity6.63–8.62%IACS
Galvanic potential-0.5–-0.42V

AISI 5140 Oil Quenched & Tempered at 540°C Magnetic properties

Magnetic typeMagnetic

AISI 5140 Oil Quenched & Tempered at 540°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5160–5260m/s
Mechanical loss coefficient (tan delta)4e-4–5.1e-4 

AISI 5140 Oil Quenched & Tempered at 540°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed17.1 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.637 – 0.76

AISI 5140 Oil Quenched & Tempered at 540°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 5140 Oil Quenched & Tempered at 540°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 5140 Oil Quenched & Tempered at 540°C Standards with similar compositions

Argentina: IRAM 5140 to IAS
Australia: 5140 to AS 1440, 5140 to AS 1444, 51B40 to AS 1444, En18 to AS G18, En18D to AS G18
Belgium: 37Cr4 to NBN 251
China: 40Cr to GB/T 11251
Czech Republic: 14140 to CSN 414140
France: 38C4 to AFNOR NF A35-552, 38C4 to AFNOR NF A35-553, 38C4 to AFNOR NF A35-556, 38C4TS to AFNOR NF A35-563, 38Cr4 to AFNOR NF A35-552, 38Cr4 to AFNOR NF A35-553, 38Cr4 to AFNOR NF A35-557, 42C4 to AFNOR NF A35-552, 42C4 to AFNOR NF A35-556, 42C4 to AFNOR NF A35-557, 45C4 to AFNOR NF A35-553, 45C4 to AFNOR NF A35-571
Germany: 1.7035 to DIN 1652, 1.7035 to DIN EN 10083, 41Cr4 to DIN 1652, 41Cr4 to DIN EN 10083
Hungary: Cr3 to MSZ 61, Cr3Z to MSZ 6251
India: 40Cr1 to IS 1570, 40Cr1 to IS 4368, 40Cr4 to IS 11169/1, 40Cr4 to IS 11185, 40Cr4 to IS 13352, 40Cr4 to IS 1570/4, 40Cr4 to IS 3930, 40Cr4 to IS 7494, 40Cr4 to IS 9175/21
International: 3 to ISO 683-7, 37Cr4 to ISO 683-1, 37Cr4 to ISO 683-18, 3a to ISO 683-7, 41Cr4 to ISO 683-1, 41Cr4 to ISO 683-18, 41Cr4E to ISO 4954, 41CrS4 to ISO 683-1, 41CrS4 to ISO 683-18
Italy: 38Cr4 to UNI 8551, 38Cr4KB to UNI 7282, 38Cr4KB to UNI 7356, 41Cr4 to UNI 7874
Japan: SCr4H to JIS G4052
Mexico: 5140 to NMX-B-203-SCFI, 5140 to NMX-B-300, 5140H to NMX-B-268, 5140H to NMX-B-300
Pan America: 5140 to COPANT 334
Romania: 37Cr10 to STAS 11500/2, 40BCr10 to STAS 791, 40Cr10 to STAS 791, 40Cr10S to STAS 791, 40Cr10X to STAS 791, 40Cr10XS to STAS 791
South Korea: SCr 440 H to KS D 3754, SCr 440 to KS D 3707
Spain: 38Cr3 to UNE 36012, 38Cr4 to UNE 36012, 38Cr4DF to UNE 36034, F.1200 to UNE 36012, F.1201 to UNE 36012
Sweden: 2245 to SS 142245
UK: 3/1 to BS 3111/1, 3/2 to BS 3111/1, 41Cr4 to BS EN 10083-1, 41Cr4 to BS EN 10250-3, 41Cr4 to BS EN 10297-1, 50H40 to BS 970/1
USA: 5140 to ASTM A29/A29M, 5140 to ASTM A331-95, 5140 to ASTM A519, 5140 to ASTM A866, 5140 to SAE J404, G51400 to ASTM A1031, G51400 to ASTM A506, UNS G51400, UNS H51400
Tradenames: A-1200, A-1201, A-1202, ALPINE HMV25, ALPINE MAC, BOCHUMER CBVZ, BSO SPEZIAL, CREUSOT 1F3/4, FIRTH-BROWN CCRF, FORTUNA TC4 SPEC, SHARON 5100 SERIES B, TKS 41CR 4, VR-40