17-4PH or 15-5PH? This 17-4PH vs 15-5PH comparison puts the two grades side by side using only the values in our 17-4PH and 15-5PH material data sheets: chemical composition, yield strength, tensile strength, hardness, elongation, fracture toughness, fatigue strength and machining speed, condition by condition. Differences are calculated from the mid-point of each range and show 15-5PH relative to 17-4PH.
Both grades are compared in the same seven aging conditions, from H900 (aged at 482°C, highest strength) to H1150M (double aged, softest). Hardness is compared in Rockwell C, because the Vickers hardness in these data sheets is given as one wide range for all conditions. Data note: the 17-4PH H1150M data sheet lists a fracture toughness of 29.7–36.3 MPa·m0.5, far below the 17-4PH H1150 value and the 15-5PH H1150M value. It is shown as given in the data sheet, but it is left out of the average differences below.
17-4PH vs 15-5PH Chemical Composition
| Element (%) | 17-4PH | 15-5PH |
|---|---|---|
| C | 0–0.07 | 0–0.07 |
| Cr | 15–17.5 | 14–15.5 |
| Ni | 3–5 | 3.5–5.5 |
| Cu | 3–5 | 2.5–4.5 |
| Nb | 0.15–0.4 | 0.15–0.4 |
| Mn | 0–1 | 0–1 |
| Si | 0–1 | 0–1 |
| P | 0–0.04 | 0–0.04 |
| S | 0–0.03 | 0–0.03 |
17-4PH vs 15-5PH Yield strength
| Condition | 17-4PH (MPa) | 15-5PH (MPa) | 15-5PH vs 17-4PH |
|---|---|---|---|
| H900 | 1170–1300 | 1170–1300 | +0% |
| H925 | 1070–1180 | 1070–1180 | +0% |
| H1025 | 1000–1110 | 986–1090 | -2% |
| H1075 | 862–986 | 862–953 | -2% |
| H1100 | 793–876 | 793–876 | +0% |
| H1150 | 690–793 | 724–800 | +3% |
| H1150M | 517–572 | 517–571 | -0% |
17-4PH 15-5PH. Dark bar = minimum, light bar = maximum of the range.
17-4PH vs 15-5PH Tensile strength
| Condition | 17-4PH (MPa) | 15-5PH (MPa) | 15-5PH vs 17-4PH |
|---|---|---|---|
| H900 | 1310–1450 | 1310–1450 | +0% |
| H925 | 1170–1300 | 1170–1300 | +0% |
| H1025 | 1070–1180 | 1060–1170 | -1% |
| H1075 | 986–1100 | 1000–1110 | +1% |
| H1100 | 965–1070 | 965–1070 | +0% |
| H1150 | 862–1020 | 931–1030 | +4% |
| H1150M | 793–876 | 793–876 | +0% |
17-4PH vs 15-5PH Hardness
| Condition | 17-4PH (HRC) | 15-5PH (HRC) | 15-5PH vs 17-4PH |
|---|---|---|---|
| H900 | 41–47 | 42–47 | +1% |
| H925 | 40–45 | 39–44 | -2% |
| H1025 | 36–41 | 38–42 | +4% |
| H1075 | 31–37 | 31–38 | +1% |
| H1100 | 33–37 | 32–37 | -1% |
| H1150 | 28–35 | 28–36 | +2% |
| H1150M | 29–33 | 27–31 | -6% |
17-4PH vs 15-5PH Elongation
| Condition | 17-4PH (%) | 15-5PH (%) | 15-5PH vs 17-4PH |
|---|---|---|---|
| H900 | 13.9–16.1 | 13–15.1 | -6% |
| H925 | 14.3–16.7 | 13–15.1 | -9% |
| H1025 | 14.8–17.2 | 13.9–16.1 | -6% |
| H1075 | 15.7–18.3 | 14.8–17.2 | -6% |
| H1100 | 17.1–19.9 | 15.7–18.3 | -8% |
| H1150 | 18.5–21.5 | 17.6–20.4 | -5% |
| H1150M | 20.4–23.7 | 20.4–23.7 | +0% |
17-4PH vs 15-5PH Fracture toughness
| Condition | 17-4PH (MPa·m0.5) | 15-5PH (MPa·m0.5) | 15-5PH vs 17-4PH |
|---|---|---|---|
| H900 | 47.3–57.8 | 79.7–97.4 | +69% |
| H925 | 78.3–95.7 | 83.7–102 | +7% |
| H1025 | 116–142 | 99.1–121 | -15% |
| H1075 | 130–158 | 107–130 | -18% |
| H1100 | 138–168 | 121–147 | -12% |
| H1150 | 161–197 | 134–164 | -17% |
| H1150M | 29.7–36.3 | 273–333 | +818% |
17-4PH vs 15-5PH Fatigue strength at 107 cycles
| Condition | 17-4PH (MPa) | 15-5PH (MPa) | 15-5PH vs 17-4PH |
|---|---|---|---|
| H900 | 364–542 | 364–542 | +0% |
| H925 | 364–542 | 364–542 | +0% |
| H1025 | 364–542 | 364–542 | +0% |
| H1075 | 364–542 | 364–542 | +0% |
| H1100 | 364–542 | 364–542 | +0% |
| H1150 | 364–542 | 364–542 | +0% |
| H1150M | 364–542 | 364–542 | +0% |
17-4PH vs 15-5PH Machining speed
| Condition | 17-4PH (m/min) | 15-5PH (m/min) | 15-5PH vs 17-4PH |
|---|---|---|---|
| H900 | 12.2 | 12.2 | +0% |
| H925 | 12.8 | 12.8 | +0% |
| H1025 | 13.4 | 13.1 | -2% |
| H1075 | 13.7 | 13.4 | -2% |
| H1100 | 13.7 | 13.7 | +0% |
| H1150 | 14.3 | 14 | -2% |
| H1150M | 14.9 | 14.9 | +0% |
17-4PH vs 15-5PH Weldability, Processing and Corrosion
| Property | 17-4PH | 15-5PH |
|---|---|---|
| Pitting resistance equivalent number (PREN) | 15–17.5 | 14–15.5 |
| Stress corrosion cracking (H900) | Slightly susceptible | Slightly susceptible |
| Stress corrosion cracking (H1150) | Susceptible | Not susceptible |
| Sea water | Restricted | Restricted |
| Weldability | Good | Good |
| Metal cold forming | Limited use | Limited use |
| Carbon equivalency | 0.65–0.97 | 0.608–0.895 |
17-4PH vs 15-5PH: Key Differences
Tensile strength is practically the same for 17-4PH and 15-5PH (average difference +1% across 7 matched conditions). Yield strength is practically the same for 17-4PH and 15-5PH (average difference +0% across 7 matched conditions). Fracture toughness depends on the condition: 15-5PH is 69% tougher than 17-4PH in H900, but 18% less tough in H1075. Machining speed is practically the same for 17-4PH and 15-5PH (average difference -1% across 7 matched conditions). On average across 7 matched conditions, 15-5PH has 6% lower elongation than 17-4PH.
17-4PH vs 15-5PH FAQ
No, in our data sheets the strength is practically the same in every matched condition. At H900 both have a yield strength of 1170–1300 MPa and tensile strength of 1310–1450 MPa.
At H900, yes: 15-5PH has a fracture toughness of 79.7–97.4 MPa·m^0.5 vs 47.3–57.8 for 17-4PH. In the H1025 to H1150 conditions, however, 17-4PH shows the higher values in our data sheets.
17-4PH contains 15–17.5% chromium and 3–5% nickel; 15-5PH contains 14–15.5% chromium and 3.5–5.5% nickel. Copper is 3–5% vs 2.5–4.5%.
Our data sheets give a PREN of 15–17.5 for 17-4PH and 14–15.5 for 15-5PH, and the same ratings for sea water (Restricted) and humidity/water.
In our data sheets 17-4PH H900 is 41–47 HRC and 17-4PH H1150 is 28–35 HRC.
17-4PH and 15-5PH Material Data Sheets
17-4PH H900 | 17-4PH H925 | 17-4PH H1025 | 17-4PH H1075 | 17-4PH H1100 | 17-4PH H1150 | 17-4PH H1150M | All 17-4PH conditions
15-5PH H900 | 15-5PH H925 | 15-5PH H1025 | 15-5PH H1075 | 15-5PH H1100 | 15-5PH H1150 | 15-5PH H1150M | All 15-5PH conditions