AISI 4140 vs 4340 Steel: Composition, Strength, Toughness and Machinability Compared

AISI 4140 or AISI 4340? This AISI 4140 vs AISI 4340 comparison puts the two grades side by side using only the values in our AISI 4140 and AISI 4340 material data sheets: chemical composition, yield strength, tensile strength, hardness, elongation, fracture toughness, fatigue strength and machining speed, condition by condition. Differences are calculated from the mid-point of each range and show AISI 4340 relative to AISI 4140.

Both grades are compared in the same conditions: annealed, normalized, and oil quenched and tempered at 205, 315, 425, 540 and 650°C. AISI 4340 adds about 1.65–2% nickel to a chromium-molybdenum base similar to AISI 4140 (see the composition table).

AISI 4140 vs AISI 4340 Chemical Composition

Element (%)AISI 4140AISI 4340
C0.38–0.430.38–0.43
Mn0.75–10.6–0.8
Si0.15–0.350.15–0.3
Cr0.8–1.10.7–0.9
Mo0.15–0.250.2–0.3
Ni—1.65–2
P0–0.0350–0.035
S0–0.040–0.04

AISI 4140 vs AISI 4340 Yield strength

ConditionAISI 4140 (MPa)AISI 4340 (MPa)AISI 4340 vs AISI 4140
Annealed370–460420–525+14%
Normalized595–715770–950+31%
Oil Q&T 205°C1480–18101510–1850+2%
Oil Q&T 315°C1290–15801430–1750+11%
Oil Q&T 425°C1020–12601230–1500+20%
Oil Q&T 540°C750–920965–1190+29%
Oil Q&T 650°C595–715770–940+31%

AISI 4140   AISI 4340. Dark bar = minimum, light bar = maximum of the range.

AISI 4140 vs AISI 4340 Yield strength (MPa)4140 Annealed370–4604340 Annealed420–5254140 Normalized595–7154340 Normalized770–9504140 Oil Q&T 205°C1480–18104340 Oil Q&T 205°C1510–18504140 Oil Q&T 315°C1290–15804340 Oil Q&T 315°C1430–17504140 Oil Q&T 425°C1020–12604340 Oil Q&T 425°C1230–15004140 Oil Q&T 540°C750–9204340 Oil Q&T 540°C965–11904140 Oil Q&T 650°C595–7154340 Oil Q&T 650°C770–940

AISI 4140 vs AISI 4340 Tensile strength

ConditionAISI 4140 (MPa)AISI 4340 (MPa)AISI 4340 vs AISI 4140
Annealed595–720670–820+13%
Normalized915–11301150–1410+25%
Oil Q&T 205°C1600–19501580–2070+3%
Oil Q&T 315°C1400–17101550–1990+14%
Oil Q&T 425°C1120–13801320–1620+18%
Oil Q&T 540°C855–10501050–1300+23%
Oil Q&T 650°C680–840865–1070+27%
AISI 4140 vs AISI 4340 Tensile strength (MPa)4140 Annealed595–7204340 Annealed670–8204140 Normalized915–11304340 Normalized1150–14104140 Oil Q&T 205°C1600–19504340 Oil Q&T 205°C1580–20704140 Oil Q&T 315°C1400–17104340 Oil Q&T 315°C1550–19904140 Oil Q&T 425°C1120–13804340 Oil Q&T 425°C1320–16204140 Oil Q&T 540°C855–10504340 Oil Q&T 540°C1050–13004140 Oil Q&T 650°C680–8404340 Oil Q&T 650°C865–1070

AISI 4140 vs AISI 4340 Hardness

ConditionAISI 4140 (HV)AISI 4340 (HV)AISI 4340 vs AISI 4140
Annealed183–223200–245+10%
Normalized275–335325–405+20%
Oil Q&T 205°C455–565465–575+2%
Oil Q&T 315°C400–490435–535+9%
Oil Q&T 425°C335–410385–475+15%
Oil Q&T 540°C260–320325–400+25%
Oil Q&T 650°C210–260255–315+21%
AISI 4140 vs AISI 4340 Hardness (HV)4140 Annealed183–2234340 Annealed200–2454140 Normalized275–3354340 Normalized325–4054140 Oil Q&T 205°C455–5654340 Oil Q&T 205°C465–5754140 Oil Q&T 315°C400–4904340 Oil Q&T 315°C435–5354140 Oil Q&T 425°C335–4104340 Oil Q&T 425°C385–4754140 Oil Q&T 540°C260–3204340 Oil Q&T 540°C325–4004140 Oil Q&T 650°C210–2604340 Oil Q&T 650°C255–315

AISI 4140 vs AISI 4340 Elongation

ConditionAISI 4140 (%)AISI 4340 (%)AISI 4340 vs AISI 4140
Annealed20–3117–27-14%
Normalized13.5–21.59–15-31%
Oil Q&T 205°C6–108–12+25%
Oil Q&T 315°C7–118–12+11%
Oil Q&T 425°C10–168–12-23%
Oil Q&T 540°C14–2210–16-28%
Oil Q&T 650°C17–2715–23-14%

AISI 4140 vs AISI 4340 Fracture toughness

ConditionAISI 4140 (MPa·m0.5)AISI 4340 (MPa·m0.5)AISI 4340 vs AISI 4140
Annealed76–12073–118-3%
Normalized68–10757–96-13%
Oil Q&T 205°C24–4844–66+53%
Oil Q&T 315°C29–5425–52-7%
Oil Q&T 425°C36–6379–91+72%
Oil Q&T 540°C45–7437–64-15%
Oil Q&T 650°C50–8044–72-11%
AISI 4140 vs AISI 4340 Fracture toughness (MPa√m)4140 Annealed76–1204340 Annealed73–1184140 Normalized68–1074340 Normalized57–964140 Oil Q&T 205°C24–484340 Oil Q&T 205°C44–664140 Oil Q&T 315°C29–544340 Oil Q&T 315°C25–524140 Oil Q&T 425°C36–634340 Oil Q&T 425°C79–914140 Oil Q&T 540°C45–744340 Oil Q&T 540°C37–644140 Oil Q&T 650°C50–804340 Oil Q&T 650°C44–72

AISI 4140 vs AISI 4340 Fatigue strength at 107 cycles

ConditionAISI 4140 (MPa)AISI 4340 (MPa)AISI 4340 vs AISI 4140
Annealed297–341300–330-1%
Normalized402–465472–545+17%
Oil Q&T 205°C593–684589–712+2%
Oil Q&T 315°C540–622581–693+10%
Oil Q&T 425°C463–535519–600+12%
Oil Q&T 540°C383–442442–513+16%
Oil Q&T 650°C326–379386–448+18%

AISI 4140 vs AISI 4340 Machining speed

ConditionAISI 4140 (m/min)AISI 4340 (m/min)AISI 4340 vs AISI 4140
Annealed2521.3-15%
Normalized15.812.2-23%
Oil Q&T 205°C8.848.23-7%
Oil Q&T 315°C10.48.84-15%
Oil Q&T 425°C12.810.4-19%
Oil Q&T 540°C16.812.8-24%
Oil Q&T 650°C21.316.2-24%

AISI 4140 vs AISI 4340 Weldability, Processing and Corrosion

PropertyAISI 4140AISI 4340
WeldabilityGoodGood
Carbon equivalency0.695–0.8670.77–0.937

AISI 4140 vs AISI 4340: Key Differences

On average across 7 matched conditions, AISI 4340 has 18% higher tensile strength than AISI 4140. On average across 7 matched conditions, AISI 4340 has 20% higher yield strength than AISI 4140. Fracture toughness depends on the condition: AISI 4340 is 72% tougher than AISI 4140 in Oil Q&T 425°C, but 15% less tough in Oil Q&T 540°C. On average across 7 matched conditions, AISI 4340 has 18% lower machining speed than AISI 4140. On average across 7 matched conditions, AISI 4340 has 11% lower elongation than AISI 4140.

AISI 4140 vs 4340 FAQ

Is 4340 stronger than 4140?

Yes. Across 7 matched conditions in our data sheets (annealed, normalized and oil quenched and tempered at 205–650°C), AISI 4340 has on average about 18% higher tensile strength and 20% higher yield strength than AISI 4140.

Is 4340 tougher than 4140?

It depends on the condition. In our data AISI 4340 has 72% higher fracture toughness in the Q&T 425°C condition but 15% lower in the Q&T 540°C condition.

What is the difference between 4140 and 4340 composition?

AISI 4340 contains 1.65–2% nickel, while AISI 4140 has no nickel listed in our data sheet. Carbon is the same in both, 0.38–0.43%.

Is 4340 harder to machine than 4140?

Yes. On average across the matched conditions, AISI 4340 has about 18% lower machining speed. Annealed: 25 m/min for 4140 vs 21.3 m/min for 4340.

AISI 4140 and AISI 4340 Material Data Sheets

AISI 4140 Annealed | AISI 4140 Normalized | AISI 4140 Oil Quenched & Tempered at 205°C | AISI 4140 Oil Quenched & Tempered at 315°C | AISI 4140 Oil Quenched & Tempered at 425°C | AISI 4140 Oil Quenched & Tempered at 540°C | AISI 4140 Oil Quenched & Tempered at 650°C | All AISI 4140 conditions

AISI 4340 Annealed | AISI 4340 Normalized | AISI 4340 Oil Quenched & Tempered at 205°C | AISI 4340 Oil Quenched & Tempered at 315°C | AISI 4340 Oil Quenched & Tempered at 425°C | AISI 4340 Oil Quenched & Tempered at 540°C | AISI 4340 Oil Quenched & Tempered at 650°C | All AISI 4340 conditions

Need AISI 4140 or AISI 4340 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.