AISI 1095 Water Quenched & Tempered at 315°C Material Data Sheet

AISI 1095 Water Quenched & Tempered at 315°C Material Data Sheet

AISI 1095 Water Quenched & Tempered at 315°C Overview

AISI 1095 water quenched tempered 315°C is AISI 1095 high carbon steel (UNS G10950) in the water quenched & tempered at 315°C condition. This AISI 1095 water quenched tempered 315°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1095 conditions in our AISI 1095 yield, tensile and hardness comparison. Looking for AISI 1095 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1095 steel parts in-house and inspects them before shipment.

AISI 1095 Water Quenched & Tempered at 315°C Designation

AISI 1095
ConditionTempered at 315°C & water quenched
UNS numberG10950
US nameASTM 1095, ASME G10950
EN name~HS95

AISI 1095 Water Quenched & Tempered at 315°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 1095 Water Quenched & Tempered at 315°C Composition detail

C (carbon)0.9–1.03%
Fe (iron)98.4–98.8%
Mn (manganese)0.3–0.5%
P (phosphorus)0–0.04%
S (sulfur)0–0.05%

AISI 1095 Water Quenched & Tempered at 315°C Physical properties

Density7.8–7.9g/cm3

AISI 1095 Water Quenched & Tempered at 315°C Mechanical properties

Young’s modulus200–215GPa
Specific stiffness25.5–27.4MN.m/kg
Yield strength (elastic limit)925–1140MPa
Tensile strength1310–1620MPa
Specific strength118–145kN.m/kg
Elongation9–13% strain
Compressive strength925–1140MPa
Flexural modulus200–215GPa
Flexural strength (modulus of rupture)925–1140MPa
Shear modulus77–84GPa
Bulk modulus155–175GPa
Poisson’s ratio0.285–0.295 
Shape factor23
Hardness – Vickers490–580HV
Elastic stored energy (springs)2080–3110kJ/m3
Fatigue strength at 10^7 cycles517–599MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
451–687MPa

AISI 1095 Water Quenched & Tempered at 315°C Impact & fracture properties

Fracture toughness28–50MPa.m0.5
Toughness (G)4.03–11.3kJ/m2

AISI 1095 Water Quenched & Tempered at 315°C Thermal properties

Melting point1290–1470°C
Maximum service temperature273–305°C
Minimum service temperature-23–7°C
Thermal conductivity47–52W/m.°C
Specific heat capacity440–480J/kg.°C
Thermal expansion coefficient11–13.5µstrain/°C
Thermal shock resistance351–471°C
Thermal distortion resistance3.62–4.54MW/m
Latent heat of fusion270–275kJ/kg

AISI 1095 Water Quenched & Tempered at 315°C Electrical properties

Electrical resistivity17–20µohm.cm
Electrical conductivity8.62–10.1%IACS
Galvanic potential-0.51–-0.43V

AISI 1095 Water Quenched & Tempered at 315°C Magnetic properties

Magnetic typeMagnetic

AISI 1095 Water Quenched & Tempered at 315°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5050–5240m/s
Mechanical loss coefficient (tan delta)3e-4–3.9e-4 

AISI 1095 Water Quenched & Tempered at 315°C Processing properties

Metal castingUnsuitable
Metal cold formingLimited use
Metal hot formingLimited use
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed8.84 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.95 – 1.11

AISI 1095 Water Quenched & Tempered at 315°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 1095 Water Quenched & Tempered at 315°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Susceptible

AISI 1095 Water Quenched & Tempered at 315°C Standards with similar compositions

Mexico: 1086 to NMX-B-301, 1095 to NMX-B-301
Pan America: 1095 to COPANT 330, 1095 to COPANT 331
UK: 060A96 to BS 970/1
USA: 1086, 1086 to ASTM A29/A29M, 1086 to ASTM A568/A568M, 1086 to ASTM A713, 1086 to SAE J1249, 1086 to SAE J403, 1095, 1095 to ASTM A29/A29M, 1095 to ASTM A568/A568M, 1095 to ASTM A713, 1095 to MIL-S-7947A, 1095 to SAE J403, 7304 to AMS 7304, C10 to MIL-S-16788A, C1095 to FED QQ-S-700D, G10860 to ASTM A510/A510M, G10950 to ASTM A510/A510M, G10950 to ASTM A576-90b, UNS G10860, UNS G10860 to UNS, UNS G10950, UNS G10950 to UNS
Tradenames: ACHORN STANDARD CARBON, AIRCO NO. 85, AQUATOUGH 100, ATLAS REFINED-10, BEST, CARR’S QUALITY RED LABEL, CHANNELER, COPPCO EXTRA, CORINTH, DISSTON NO. 5190, EIS-V3, ELECTREX, FAGERSTA OVERCOAT AXE, FAGERSTA REGULAR, FAGERSTA SPECIAL, FIRTH-BROWN F95C, FORTUNA GSB10, FORTUNA W93, G.W. REGULAR, G.W. SPECIAL, H S C COLD HEADER, H S C REGULAR, JESSOP BLUE LABEL, JESSOP SHEET SPRING, K.E.A. 108, MARREL MO, MCINNES FOLDIER DIE, PAGE HIGH CARBON, PREMIER HC WELD, RED SEAL DIE STEEL, S/100, SAVILLE BEST CAST STEEL, SAVILLE CAST, SAVILLE CAST STEEL WARRANTED, SOLID DRILL, SPRING STEEL, STANDARD, TRU-COR DRILL ROD, TULIPE EXTRA NO. 3, UNA NO. 325, WHELCO STD