Common Trade Names for Zinc-Flake Coatings

Common Trade Names for Zinc-Flake Coatings

Trade NameManufacturer / OwnerNotes
GeometNOF Metal Coatings GroupCr-free; most widely OEM-approved worldwide
DacrometNOF Metal Coatings GroupOlder generation; contains Cr(VI) unless specified Cr-free
GeoBlackNOF Metal CoatingsBlack variant of Geomet; mainly used for automotive appearance parts
Plus (e.g., GEOMET 500 PLUS)NOFEnhanced friction & topcoat systems
Tyrogalv / Schmid Zinc FlakeAtotech / Doerken SchmidGerman manufacturer; automotive approvals
ZintekAtotechGeneric zinc-flake product line
ZingaFlake / Zinga SystemsZinga MetMostly corrosion-protection systems incl. zinc-rich
Zircotec ZF coatingsZircotecHigh-performance variants (less common for fasteners)
ZinKladMacDermid EnthoneOEM-approved coating systems (includes zinc-flake)
JS500 / JS600 (Japan)Yamato / Japanese aplicatorsCommon in Asian automotive supply chains
Ruspert / Ruspert-SNofmet / Metal Coatings JapanTri-coat zinc-flake & ceramic system
Magni (e.g., Magni 565, Magni 575)Magni Coatings (USA)One of the largest competitors to Geomet; widely OEM-approved
Delta-MagniJoint programsUsed by US and Asian OEMs
ZFA CoatingsChinese manufacturersWidely used in industrial fasteners
Dörken Delta-Protekt (e.g., Delta Protekt KL100, GZ series)Dörken Coatings (Germany)Leading zinc-flake brand in EU automotive

Zinc-Flake Coatings – Full Comparison Quick Guide

Brand / Trade nameTypical types / gradesAppearance / ColorSalt spray (typ.)Thickness (typ.)Top-coat available?Notes / OEM / spec
GEOMET (NOF)321, 360, 500 (500A/500B), 720, 430Silver-gray; GEOBLACK variants = black. 480-1500+ h depending on grade/topcoat (321 ≈720 h, 500 ≈720-1000 h, 720 >1000 h). ~5-15 μm (adjustable by grade/process). Yes – PLUS / GEOKOTE topcoats (lubricant / colour / friction tuning). (cdn.simplifiedbuilding.com)Widely OEM-approved (VW, Toyota, Ford etc.); chromate-free variants available. (Nof Metal Coatings)
GEO-BLACK (NOF)GEOBLACK 500M, ML, 180Black (matte → semi-gloss). ~720-2000 h depending on system & topcoat (manufacturer data quotes wide range). 8-15 μm typical. Yes – black organic topcoats (PLUS black, GEOKOTE). Designed for appearance + corrosion; controlled μ per ISO 16047.
DACROMET (legacy; NOF products also promoted)DACROMET 320, 500 (legacy and modern variants)Silver / dull grey (older chromated types existed). ~240-1000 h (legacy sheets: typical ≥ 500-600 h; depends on grade). ~7-13 μm typical. Yes – friction/topcoat options for torque control. Historically used widely in automotive; modern equivalents offered Cr-free to meet regulations.
MAGNI (Magni Coatings / Magni 565 family)MAGNI 565, 575, 590 etc.Silver; some black topcoat versions~480-1000 h (Magni 565 datasheets show 480-1000 h; some docs claim 1000 h). ~5-13 μm (many fastener specs show 5-13 μm). (Magni Coatings)Yes – duplex (inorganic base + organic topcoat) common. Magni 565 is widely OEM-specified (many OEM approvals listed in data sheets). (SWD, Inc.)
DÖRKEN / DELTA-PROTECT (Delta-Protekt)Delta-Protect KL series (KL100 etc.)Silver / grey; variants with topcoats~480-1500 h (product-dependent). ~5-15 μmYes – Delta Seal, Delta Tone topcoatsLeading EU zinc-flake family; OEM approvals common.
ZINTEK (Atotech / Tyrogalv family)Zintek / Tyrogalv / Schmid zinc-flake linesSilver gray~480-1000 h typical (varies by product)~5-12 μmYes – topcoat / lubricant optionsAtotech / Schmid products are used in automotive & industrial markets.
TYROGALV / Schmid Zinc-FlakeTyrogalv familySilver / greyTypical OEM ranges (480-1000 h)~5-12 μmYesGerman suppliers-automotive approvals common.
MAGNI / DELTA hybrids (other regional brands)Magni family, regional variantsSilver / black options480-1000 h typical5-15 μmYesOften marketed as OEM-equivalent to GEOMET.
ZINGAFLAKE / Zinga systemsZingaFlake, Zinga systemsSilver / grey (zinc-rich)varies; marketed as high corrosion protection (check datasheet)variesYes (topcoats)Zinga family focused on large-area corrosion protection (not only fasteners).
ZFA (Chinese suppliers / generic zinc-flake)ZFA-xxx seriesSilver / grey~480-1000 h (vendor dependent)~6-15 μmYes (vendor options)Widely used in industrial fasteners; verify OEM acceptance per buyer.
ZINCLAD / ZinKlad (MacDermid / Enthone lines)ZinKlad variantsSilver / greyvaries (covering fastener market)~5-12 μmYesMacDermid products include zinc-flake families with OEM approvals.
ZIRCOTEC ZF (high-performance)ZF / Zircotec variantsGrey / specialized finishes≥720-1000 h (per product)~8-15 μmYes (PTFE / ceramic options)Specialty, high-temp or friction-controlled types (less common for general fasteners).
JS-series (Japan: JS500 / JS600)JS500, JS600Silver / grey~600-1000 h typical (OEM specs in Asia)~6-12 μmYesCommon in Japanese supply chains; used by Toyota, Honda suppliers.
RUSPERT (Ruspert)Ruspert / Ruspert-SSilver / black variants~480-1000 h (product dependent)~5-15 μmYesMarketed as Cr-free alternatives in some regions.
Zinc-flake + PTFE / GEOKOTE / GEOKOTE-styleGEOKOTE, PTFE black topcoatsBlack / graphite-like~1000-1500+ h (with right basecoat)10-18 μm (multi-layer)Topcoat is the key featureFor low friction, chemical resistance & aesthetic black finish.