Steel Tempering Chart: Hardness and Tensile Strength of Carbon and Alloy Steels at 205–650°C

How hard and how strong will a steel be after quenching and tempering at a given temperature? This tempering chart compares 30 oil quenched and 6 water quenched carbon and low alloy steels tempered at 205, 315, 425, 540 and 650°C, side by side. Every value is taken from our individual material data sheets, and every cell links to its source data sheet.

Use it to pick a grade and tempering temperature for a target hardness or tensile strength, or to see how much strength a grade keeps at higher tempering temperatures where toughness and ductility improve.

Tempering Chart: Hardness of Oil Quenched Steels by Tempering Temperature

Hardness vs tempering temperature, oil quenched (HV, mid-point of range)180300420540659205°C315°C425°C540°C650°C4340516010951340863041401040
Grade205°C (HV)315°C (HV)425°C (HV)540°C (HV)650°C (HV)
AISI 1040240–290235–285220–270195–240180–220
AISI 1050—290–360250–310240–290205–250
AISI 1060290–360290–360280–350250–310210–260
AISI 1080360–420360–420350–410300–350240–280
AISI 1095370–430350–410335–395300–350250–300
AISI 1137320–390260–320240–290210–260183–223
AISI 1141415–505375–455300–370240–290200–245
AISI 1144255–305240–290230–280215–265200–245
AISI 1340455–555408–498340–415270–330230–280
AISI 4037280–345270–330248–303225–275203–248
AISI 4042465–568410–500343–423275–335220–270
AISI 4140455–565400–490335–410260–320210–260
AISI 4150475–585445–545395–485335–410265–325
AISI 4340465–575435–535385–475325–400255–315
AISI 5046430–530360–440305–375255–315215–265
AISI 50B46—455–555365–445290–360250–305
AISI 50B60—470–575390–480315–385260–320
AISI 5130425–525395–485340–420280–340225–275
AISI 5140440–540405–495330–405255–315215–265
AISI 5150470–580425–525370–450310–380248–303
AISI 5160563–693500–610415–505305–375248–303
AISI 6150483–593433–533378–463310–380253–313
AISI 81B45495–605425–525363–448305–375255–315
AISI 8630415–515385–475340–415280–345220–270
AISI 8640—415–505360–443308–378255–315
AISI 86B45470–580425–525355–438303–373255–315
AISI 8650470–580440–540375–465305–375250–310
AISI 8740518–638445–545370–460325–405275–335
AISI 9255540–660518–638428–528318–393260–320
AISI 94B30425–525400–490345–425275–345228–283

Tempering Chart: Tensile Strength of Oil Quenched Steels by Tempering Temperature

Tensile strength vs tempering temperature, oil quenched (MPa, mid-point of range)5691011145318942336205°C315°C425°C540°C650°C4340109551601340863041401040
Grade205°C (MPa)315°C (MPa)425°C (MPa)540°C (MPa)650°C (MPa)
AISI 1040700–860700–860680–835645–795565–700
AISI 1050—880–1080840–1040785–970660–815
AISI 1060990–1220990–1220965–1190865–1070720–880
AISI 10801180–14501170–14401160–14301020–1250800–980
AISI 10951160–14201130–14001090–1340980–1200805–990
AISI 1137970–1200885–1090785–970680–840590–720
AISI 11411470–18001230–15201050–1290805–990640–780
AISI 1144780–970775–965760–935725–890645–800
AISI 13401630–19901430–17501130–1400865–1070720–880
AISI 4037920–1140855–1050785–970710–875620–770
AISI 40421620–19801450–17801160–1420885–1090710–875
AISI 41401600–19501400–17101120–1380855–1050680–840
AISI 41501740–21201590–19401360–16801090–1330860–1060
AISI 43401580–20701550–19901320–16201050–1300865–1070
AISI 50461570–19201270–15501020–1260840–1040705–870
AISI 50B46—1600–19601250–1540970–1200800–965
AISI 50B60—1700–20701360–16701010–1240805–990
AISI 51301460–17801350–16501150–1410925–1140710–875
AISI 51401610–19801420–17401180–1440900–1100675–840
AISI 51501750–21401560–19201300–16001010–1240730–895
AISI 51602000–24501800–22001400–18101050–1290805–990
AISI 61501740–21301550–19001290–15901040–1280850–1040
AISI 81B451830–22401590–19501270–1550990–1220805–990
AISI 86301480–18101330–16401150–1410925–1140690–855
AISI 8640—1490–18201240–1520990–1220805–990
AISI 86B451780–21801530–18701240–1520990–1220810–995
AISI 86501740–21401550–19001300–16001060–1290865–1070
AISI 87401800–22001540–19001290–15801090–1330885–1090
AISI 92551890–23201740–21401450–17801130–1380890–1100
AISI 94B301550–19001440–17601210–1480900–1100740–915

Tempering Chart: Yield Strength of Oil Quenched Steels by Tempering Temperature

Grade205°C (MPa)315°C (MPa)425°C (MPa)540°C (MPa)650°C (MPa)
AISI 1040530–655530–655495–610440–540385–480
AISI 1050—645–800585–720520–640420–520
AISI 1060700–860700–860685–845600–740465–580
AISI 1080880–1080880–1080855–1050725–890540–660
AISI 1095740–915730–895690–855605–750495–610
AISI 1137840–1040755–930655–805545–670430–535
AISI 11411090–13401150–1420925–1140685–845530–655
AISI 1144560–695555–690545–680510–635450–555
AISI 13401430–17601280–15701040–1270740–915555–690
AISI 4037680–840685–845660–800595–715375–465
AISI 40421500–18201310–16001050–1300790–980620–760
AISI 41401480–18101290–15801020–1260750–920595–715
AISI 41501550–19001430–17501240–1520995–1220755–925
AISI 43401510–18501430–17501230–1500965–1190770–940
AISI 50461270–15501040–1280840–1020690–840595–715
AISI 50B46—1460–17801120–1380880–1080710–875
AISI 50B60—1600–19501240–1530900–1100700–860
AISI 51301370–16701270–15501090–1330840–1040620–760
AISI 51401480–18101300–16001050–1300770–955600–725
AISI 51501560–19001470–17501280–1440925–1140725–890
AISI 51601610–19801590–19601320–1610935–1150720–880
AISI 61501520–18601410–17401200–1470960–1180755–925
AISI 81B451550–19001410–17301180–1440920–1140710–875
AISI 86301350–16601250–15401050–1300805–990620–760
AISI 8640—1360–16701170–1430925–1140720–880
AISI 86B451490–18101400–17101190–1450925–1140785–970
AISI 86501500–18501400–17101190–1460945–1160745–910
AISI 87401490–18201400–17101220–15001020–1260810–995
AISI 92551840–22601610–19801340–1640990–1220730–895
AISI 94B301400–17101280–15701090–1330835–1030650–795

Tempering Chart: Water Quenched Steels

The data sheets below are for water quenching. Water quenching gives a faster cooling rate than oil, so compare these values only with each other or use them alongside the oil quenched tables with that in mind.

Hardness of Water Quenched Steels (HV)

Grade205°C (HV)315°C (HV)425°C (HV)540°C (HV)650°C (HV)
AISI 1030450–550360–440275–355235–285190–230
AISI 1040465–565400–490320–390250–300188–228
AISI 1050465–565400–490340–420265–325215–265
AISI 1095550–650490–580360–430265–325220–260
AISI 1137375–455340–415280–350240–290173–213
AISI 4130420–515390–480345–420285–355225–275

Tensile Strength of Water Quenched Steels (MPa)

Grade205°C (MPa)315°C (MPa)425°C (MPa)540°C (MPa)650°C (MPa)
AISI 1030760–935720–880655–810600–740525–650
AISI 1040805–990800–985755–925700–860600–740
AISI 10501010–1240980–1200900–1100770–950640–795
AISI 10951340–16401310–16201230–15201030–1260755–930
AISI 11371350–16501230–1420990–1220740–915580–715
AISI 41301450–17701350–16501150–1410925–1140730–895

Which Steel and Tempering Temperature Reaches a Target Strength?

The table lists, for each minimum tensile strength target, the oil quenched grades whose data sheet minimum reaches the target, with the highest tempering temperature that still does so. A higher tempering temperature generally means better toughness and ductility at that strength.

Minimum tensile strengthOil quenched grades (highest tempering temperature reaching it)
≥ 800 MPa1050 (425°C), 1060 (540°C), 1080 (650°C), 1095 (650°C), 1137 (315°C), 1141 (540°C), 1340 (540°C), 4037 (315°C), 4042 (540°C), 4140 (540°C), 4150 (650°C), 4340 (650°C), 5046 (540°C), 50B46 (650°C), 50B60 (650°C), 5130 (540°C), 5140 (540°C), 5150 (540°C), 5160 (650°C), 6150 (650°C), 81B45 (650°C), 8630 (540°C), 8640 (650°C), 86B45 (650°C), 8650 (650°C), 8740 (650°C), 9255 (650°C), 94B30 (540°C)
≥ 1000 MPa1080 (540°C), 1095 (425°C), 1141 (425°C), 1340 (425°C), 4042 (425°C), 4140 (425°C), 4150 (540°C), 4340 (540°C), 5046 (425°C), 50B46 (425°C), 50B60 (540°C), 5130 (425°C), 5140 (425°C), 5150 (540°C), 5160 (540°C), 6150 (540°C), 81B45 (425°C), 8630 (425°C), 8640 (425°C), 86B45 (425°C), 8650 (540°C), 8740 (540°C), 9255 (540°C), 94B30 (425°C)
≥ 1200 MPa1141 (315°C), 1340 (315°C), 4042 (315°C), 4140 (315°C), 4150 (425°C), 4340 (425°C), 5046 (315°C), 50B46 (425°C), 50B60 (425°C), 5130 (315°C), 5140 (315°C), 5150 (425°C), 5160 (425°C), 6150 (425°C), 81B45 (425°C), 8630 (315°C), 8640 (425°C), 86B45 (425°C), 8650 (425°C), 8740 (425°C), 9255 (425°C), 94B30 (425°C)
≥ 1400 MPa1141 (205°C), 1340 (315°C), 4042 (315°C), 4140 (315°C), 4150 (315°C), 4340 (315°C), 5046 (205°C), 50B46 (315°C), 50B60 (315°C), 5130 (205°C), 5140 (315°C), 5150 (315°C), 5160 (425°C), 6150 (315°C), 81B45 (315°C), 8630 (205°C), 8640 (315°C), 86B45 (315°C), 8650 (315°C), 8740 (315°C), 9255 (425°C), 94B30 (315°C)
≥ 1600 MPa1340 (205°C), 4042 (205°C), 4140 (205°C), 4150 (205°C), 50B46 (315°C), 50B60 (315°C), 5140 (205°C), 5150 (205°C), 5160 (315°C), 6150 (205°C), 81B45 (205°C), 86B45 (205°C), 8650 (205°C), 8740 (205°C), 9255 (315°C)

Steel Tempering Chart FAQ

Which steel is hardest after oil quenching and tempering at 205°C?

In our data sheets AISI 5160 is the hardest oil quenched grade tempered at 205°C, at 563–693 HV.

How much hardness does AISI 4140 lose when tempered at 650°C instead of 205°C?

Oil quenched AISI 4140 drops from 455–565 HV at 205°C to 210–260 HV at 650°C, and tensile strength from 1600–1950 MPa to 680–840 MPa.

Which steels keep at least 1400 MPa tensile strength when tempered at 425°C or higher?

Oil quenched grades whose data sheet minimum tensile strength is 1400 MPa or more at 425°C or higher (highest such tempering temperature in brackets): 5160 (425°C), 9255 (425°C).

Why does hardness fall as tempering temperature rises?

Tempering relieves the hard, brittle martensite formed during quenching. Higher tempering temperatures go further, lowering hardness and strength while improving ductility and toughness, as the tables above show for every grade.

Can I compare water quenched and oil quenched values directly?

Only with care. Water cools faster than oil, so water quenched data sheets show higher hardness for the same grade and tempering temperature. That is why this chart lists them in separate tables.

Related comparisons: AISI 4130 vs 4140 | AISI 4140 vs 4340 | low alloy steel grades | medium and high carbon steel grades