HASTELLOY B-2 Mechanical Properties (sheet, Nickel-molybdenum alloy)

Designation
UNS numberN10665
US nameASTM Grade N10655
EN number2.4617

Mechanical properties: HASTELLOY B-2, sheet

Young’s modulus209–223GPa
Specific stiffness22.6–24.2MN.m/kg
Yield strength (elastic limit)470–580MPa
Tensile strength865–1070MPa
Specific strength50.9–62.9kN.m/kg
Elongation40–65% strain
Compressive strength470–580MPa
Flexural modulus209–223GPa
Flexural strength (modulus of rupture)470–580MPa
Shear modulus75–90GPa
Bulk modulus170–210GPa
Poisson’s ratio0.3–0.32 
Shape factor25   
Hardness – Vickers220–280HV
Hardness – Rockwell B95–103HRB
Hardness – Rockwell C16–27HRC
Hardness – Brinell207–265HB
Elastic stored energy (springs)516–773kJ/m^3
Fatigue strength at 10^7 cycles345–535MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles318–580MPa

Impact & fracture properties: HASTELLOY B-2, sheet

Fracture toughness296–328MPa.m^0.5
Toughness (G)404–500kJ/m^2

MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey