EN 10088-1 Standard Guide

EN 10088-1 Standard Guide

Stainless steels – Part 1: List of stainless steels

1. Steel Numbering System

Steel Numbering System (EN 10027-2)
  1.40xx: < 2.50% Ni, without Mo/Nb/Ti
  1.41xx: < 2.50% Ni, with Mo, without Nb/Ti
  1.43xx: ≥ 2.50% Ni, without Mo/Nb/Ti
  1.44xx: ≥ 2.50% Ni, with Mo, without Nb/Ti
  1.45xx/1.46xx: Special additions
  1.47xx: Heat resistant, < 2.50% Ni
  1.48xx: Heat resistant, ≥ 2.50% Ni
  1.49xx: Creep resistant

2. Austenitic Stainless Steels | Corrosion Resistant Steels

Steel NameSteel NumberC max %Si max %Mn max %P max %S max %Cr range %Mo max %Ni range %N max %Cu max %Others
X10CrNi18-81.43100.030-0.152.002.000.0450.01516.0-19.00.806.0-9.50.10––
X2CrNi18-91.43070.0301.002.000.0450.01517.5-19.5–8.0-10.50.10–304L
X9CrNi18-91.43250.030-0.151.002.000.0450.03017.0-19.0–8.0-10.0–––
X8CrNiS18-91.43050.101.002.000.0450.15-0.3517.0-19.0–8.0-10.00.101.00Free machining, S for machinability
X6CrNiCuS18-9-21.45700.081.002.000.0450.15-0.3517.0-19.00.608.0-10.00.101.40-1.80Free machining
X3CrNiCu18-9-41.45670.041.002.000.0450.01517.0-19.0–8.5-10.50.103.00-4.0Cu for improved corrosion
X5CrNiN19-91.43150.061.002.000.0450.01518.0-20.0–8.0-11.00.12-0.22–N-strengthened
X3CrNiCu19-9-21.45600.0351.001.50-2.000.0450.01518.0-19.0–8.0-9.00.101.50-2.00–
X5CrNiCu19-6-21.46400.030-0.080.501.50-4.00.0450.01518.0-19.0–5.5-6.90.030-0.111.30-2.00–
X2CrNiN18-101.43110.0301.002.000.0450.01517.5-19.5–8.5-11.50.12-0.22–304LN
X5CrNi18-101.43010.071.002.000.0450.01517.5-19.5–8.0-10.50.10–304 – Most common
X2CrNiSi18-101.46820.030.80-2.02.000.0450.01517.5-19.50.40-0.809.0-11.00.10–Si for high temp oxidation
X6CrNiTi18-101.45410.081.002.000.0450.01517.0-19.0–9.0-12.0––Ti: 5×C-0.70, 321
X6CrNiNb18-101.45500.081.002.000.0450.01517.0-19.0–9.0-12.0––Nb: 10×C-1.00, 347
X2CrNiCu19-101.46500.0301.002.000.0450.01518.5-20.0–9.0-10.00.081.00–
X2CrNi19-111.43060.0301.002.000.0450.01518.0-20.0–10.0-12.00.10–304L
X4CrNi18-121.43030.061.002.000.0450.01517.0-19.0–11.0-13.00.10–305
X1CrNiSi18-15-41.43610.0153.7-4.52.000.0250.01016.5-18.50.2014.0-16.00.10–High Si
X8CrMnCuN17-8-31.45970.102.006.5-9.00.0400.03015.0-18.01.003.000.10-0.302.00-3.5Mn-bearing
X8CrMnNi19-6-31.43760.101.005.0-8.00.0450.01517.0-20.5–2.00-4.50.30–200 series
X3CrMnNiCu15-8-5-31.46150.0301.007.0-9.00.0400.01014.0-16.00.804.5-6.00.02-0.062.0-4.0–
X12CrMnNiN17-7-51.43720.151.005.5-7.50.0450.01516.0-18.0–3.5-5.50.05-0.25–201
X2CrMnNiN17-7-51.43710.0301.006.0-8.00.0450.01516.0-17.5–3.5-5.50.15-0.251.00–
X9CrMnNiCu17-8-5-21.46180.101.005.5-9.50.0700.01016.5-18.5–4.5-5.50.151.00-2.50–
X30MnCrN16-141.46780.20-0.401.0014.0-18.00.0450.01512.0-16.0––0.20-0.402.00High Mn austenitic
X12CrMnNiN18-9-51.43730.151.007.5-10.50.0450.01517.0-19.0–4.0-6.00.05-0.25–202
X8CrMnNiN18-9-51.43740.05-0.100.30-0.609.0-10.00.0350.03017.5-18.50.505.0-6.00.25-0.320.40–
X11CrNiMnN19-8-61.43690.07-0.150.50-1.005.0-7.50.0300.01517.5-19.5–6.5-8.50.20-0.30––
X13CrMnNiN18-13-21.40200.151.0011.0-14.00.0450.03016.5-19.0–0.5-2.50.20-0.45––
X6CrMnNiN18-13-31.43780.081.0011.5-14.50.0600.03017.0-19.0–2.3-3.70.20-0.40––
X6CrMnNiCuN18-12-4-21.46460.02-0.101.0010.5-12.50.0500.01517.0-19.00.503.5-4.50.20-0.301.50-3.00Patented grade*
X3CrMnNiN20-9-61.43910.0401.008.0-10.00.0450.03019.0-21.50.755.5-7.50.15-0.40––
X1CrNi25-211.43350.0200.252.000.0250.01024.0-26.00.2020.0-22.00.10–310S
X6CrNi23-131.48330.04-0.101.502.000.0450.01522.0-24.0–12.0-14.0––309
X8CrNi25-211.48450.05-0.101.502.000.0450.01524.0-26.0–19.0-22.0––310
X2CrNiMoCuS17-10-21.45980.0301.002.000.0450.10-0.2016.5-18.52.00-2.5010.0-13.00.101.30-1.80Free machining
X3CrNiCuMo17-11-3-21.45780.041.002.000.0450.01516.5-17.52.00-2.5010.0-11.00.103.0-3.5–
X2CrNiMoN17-11-21.44060.0301.002.000.0450.01516.5-18.52.00-2.5010.0-12.50.12-0.22–316LN
X2CrNiMo17-12-21.44040.0301.002.000.0450.01516.5-18.52.00-3.010.0-13.00.10–316L – Very common
X5CrNiMo17-12-21.44010.071.002.000.0450.01516.5-18.52.00-2.5010.0-13.00.10–316
X6CrNiMoTi17-12-21.45710.081.002.000.0450.01516.5-18.52.00-2.5010.5-13.5––Ti: 5×C-0.70, 316Ti
X6CrNiMoNb17-12-21.45800.081.002.000.0450.01516.5-18.52.00-2.5010.5-13.5––Nb: 10×C-1.00, 316Nb
X2CrNiMoN21-9-11.44200.0301.002.000.0450.01519.5-21.50.50-1.508.0-9.50.14-0.251.00Patented grade*
X2CrNiMo17-12-31.44320.0301.002.000.0450.01516.5-18.52.50-3.0010.5-13.00.10–316L
X3CrNiMo17-12-31.44360.051.002.000.0450.01516.5-18.52.50-3.0010.5-13.00.10–316
X3CrNiMo18-12-31.44490.0351.002.000.0450.01517.0-18.22.25-2.7511.5-12.50.081.00–
X2CrNiMoN17-13-31.44290.0301.002.000.0450.01516.5-18.52.50-3.0011.0-14.00.12-0.22–316LN
X2CrNiMoN18-12-41.44340.0301.002.000.0450.01516.5-19.53.00-4.010.5-14.00.10-0.20––
X2CrNiMo18-14-31.44350.0301.002.000.0450.01517.0-19.02.50-3.0012.5-15.00.10–317L
X2CrNiMoN17-13-51.44390.0301.002.000.0450.01516.5-18.54.0-5.012.5-14.50.12-0.22–317LMN
X2CrNiMo18-15-41.44380.0301.002.000.0450.01517.5-19.53.00-4.013.0-16.00.10–317L
X5CrNiMnMoNNbV22-12-5-21.46810.0601.004.0-6.00.0450.03020.5-23.51.5-3.011.5-13.50.20-0.40–Nb: 0.10-0.30, V: 0.10-0.30
X1CrNiMoCuN20-18-71.45470.0200.701.000.0300.01019.5-20.56.0-7.017.5-18.50.18-0.250.50-1.00254 SMO – Superaustenitic
X1CrNiMoN25-22-21.44660.0200.702.000.0250.01024.0-26.02.00-2.5021.0-23.00.10-0.16–310MoLN
X1CrNiMoCuNW24-22-61.46590.0200.702.00-4.00.0300.01023.0-25.05.5-6.521.0-23.00.35-0.501.00-2.00W: 1.50-2.50
X1CrNiMoCuN24-22-81.46520.0200.502.00-4.00.0300.00523.0-25.07.0-8.021.0-23.00.45-0.550.30-0.60654 SMO – Superaustenitic
X2CrNiMnMoN25-18-6-51.45650.0301.005.0-7.00.0300.01524.0-26.04.0-5.016.0-19.00.30-0.60–Nb: 0.15
X1NiCrMoCu31-27-41.45630.020.501.500.0250.01026.0-28.03.00-4.030.0-32.0–1.00-2.00Alloy 825 (Ni-based)
X1NiCrMoCu25-20-51.45390.020.502.000.0300.01519.0-21.04.0-5.024.0-26.0–1.20-2.00904L (Ni-based)
X1NiCrMoCuN25-20-71.45290.020.502.000.0250.01019.0-21.06.0-7.024.0-26.00.15-0.251.20-2.00Superaustenitic Ni-based

3. Austenitic-Ferritic (Duplex) Stainless Steels | Corrosion Resistant Steels

Steel NameSteel NumberC max %Si max %Mn max %P max %S max %Cr range %Mo max %Ni range %N range %Cu max %Others
X2CrMnNiSiN20-5-4-21.46700.0301.50-3.004.0-6.00.0400.01018.0-21.00.603.00-5.50.10-0.201.00Patented*
X2CrNiMoSi18-5-31.44240.0301.40-2.001.20-2.000.0350.01518.0-19.02.50-3.004.5-5.20.05-0.10–3RE60
X2CrNiMnMoCuN21-3-1-11.46370.015-0.0300.30-0.501.05-1.300.0350.0519.9-20.31.15-1.302.65-3.000.18-0.210.30-0.50Patented*
X2CrNiN23-41.43620.0301.002.000.0350.01522.0-24.50.10-0.603.5-5.50.05-0.200.10-0.602304 lean duplex
X2CrMnNiN21-5-11.41620.041.004.0-6.00.0400.01521.0-22.00.10-0.801.35-1.900.20-0.250.10-0.80LDX 2101
X2CrMnNiMoN21-5-31.44820.0301.004.0-6.00.0350.03019.5-21.50.10-0.601.50-3.500.05-0.201.00–
X2CrNiMoN22-5-31.44620.0301.002.000.0350.01521.0-23.02.50-3.54.5-6.50.10-0.22–2205 standard duplex
X2CrNiMnMoCuN24-4-3-21.46620.0300.702.50-4.00.0350.00523.0-25.01.00-2.003.00-4.50.20-0.300.10-0.80Patented*
X2CrNiMoCuN25-6-31.45070.0300.702.000.0350.01524.0-26.03.00-4.06.0-8.00.20-0.301.00-2.502507 superduplex
X3CrNiMoN27-5-21.44600.051.002.000.0350.01525.0-28.01.30-2.004.5-6.50.05-0.20––
X2CrNiMoN25-7-41.44100.0301.002.000.0350.01524.0-26.03.00-4.56.0-8.00.24-0.35–2507 superduplex
X2CrNiMoCuWN25-7-41.45010.0301.001.000.0350.01524.0-26.03.00-4.06.0-8.00.20-0.300.50-1.00W: 0.50-1.00, superduplex
X2CrNiMoN29-7-21.44770.0300.500.80-1.500.0300.01528.0-30.01.50-2.605.8-7.50.30-0.400.80Hyperduplex
X2CrNiMoCoN28-8-5-11.46580.0300.501.500.0350.01026.0-29.04.0-5.05.5-9.50.30-0.501.00Co: 0.50-2.00, hyperduplex

4. Ferritic Stainless Steels | Corrosion Resistant Steels

Steel NameSteel NumberC max %Si max %Mn max %P max %S max %Cr range %Mo max %Ni max %N max %Ti/Nb %Others
X2CrTi121.45120.0301.001.000.0400.01510.5-12.5–––Ti: 6×(C+N)-0.65409
X6CrNiTi121.45160.080.701.500.0400.01510.5-12.5–0.50-1.50–Ti: 0.05-0.35–
X6Cr131.40000.081.001.000.0400.01512.0-14.0––––410S
X6CrAl131.40020.081.001.000.0400.01512.0-14.0––––Al: 0.10-0.30, 405
X2CrMnNiTi121.46000.0301.001.00-2.500.0400.01511.0-13.0–0.30-1.000.025Ti: 6×C-0.35–
X2CrSiTi151.46300.0300.20-1.501.000.0500.05013.0-16.00.500.50–Ti: 4×(C+N)+0.15-0.80Al: 1.50
X1CrNb151.45950.0201.001.000.0250.01514.0-16.0––0.020Nb: 0.20-0.60–
X6Cr171.40160.081.001.000.0400.01516.0-18.0––––430
X2CrTi171.45200.0250.500.500.0400.01516.0-18.0––0.015Ti: 4×(C+N)+0.15-0.80–
X3CrTi171.45100.051.001.000.0400.01516.0-18.0–––Ti: 4×(C+N)+0.15-0.80430Ti
X3CrNb171.45110.051.001.000.0400.01516.0-18.0–––Nb: 12×C-1.00430Nb
X2CrNbZr171.45900.0301.001.000.0400.01516.0-17.5–––Nb: 0.35-0.55, Zr≥7×(C+N)+0.15–
X6CrNi17-11.40170.081.001.000.0400.01516.0-18.0–1.20-1.60––434
X2CrTiNb181.45090.0301.001.000.0400.01517.5-18.5–––Ti: 3×C+0.30-1.00, Nb: 0.10-0.60439
X2CrAlSiNb181.46340.0300.20-1.501.000.0500.05017.5-18.50.500.50–Nb: 3×C+0.30-1.00, Al: 0.20-1.50–
X2CrNbTi201.46070.0301.001.000.0400.01518.5-20.5––0.030Nb: 1.00, Ti: 4×(C+N)+0.15-0.80–
X2CrTi211.46110.0301.001.000.0500.05019.0-22.00.500.50–Ti: 4×(C+N)+0.20-1.00, Al: 0.05Patented*
X2CrNbCu211.46210.0301.001.000.0400.01520.0-21.5––0.030Nb: 0.20-1.00, Cu: 0.10-1.00441
X2CrCuNbTiV22-11.46220.0301.000.800.0400.01520.0-24.0––0.030Nb: 0.10-0.70, Ti: 0.10-0.70, V: 0.03-0.50Cu: 0.30-0.80, Pat*
X2CrTi241.46130.0301.001.000.0500.05022.0-25.00.500.50–Ti: 4×(C+N)+0.20-1.00, Al: 0.05Patented*
X5CrNiMoTi15-21.45890.081.001.000.0400.01513.5-15.50.20-1.201.00-2.50–Ti: 0.30-0.50–
X6CrMoS171.41050.081.501.500.0400.15-0.3516.0-18.00.20-0.60–––Free machining
X6CrMo17-11.41130.081.001.000.0400.01516.0-18.00.90-1.40–––434
X2CrMoTi17-11.45130.0251.001.000.0400.01516.0-18.00.80-1.40–0.020Ti: 4×(C+N)+0.15-0.80434
X6CrMoNb17-11.45260.081.001.000.0400.01516.0-18.00.80-1.40–0.040Nb: 7×(C+N)+0.10-1.00434
X2CrMoTi18-21.45210.0251.001.000.0400.01517.0-20.01.75-2.50–0.030Ti: 4×(C+N)+0.15-0.80444
X2CrMoTiS18-21.45230.0301.000.500.0400.15-0.3517.5-19.02.00-2.50––Ti: 4×(C+N)+0.15-0.80, (C+N)≤0.040Free machining
X2CrMoSiS18-2-11.41060.0302.501.000.0400.15-0.3517.5-19.51.50-2.500.75––Free machining
X6CrMoS19-21.41140.0801.002.500.0400.15-0.3517.5-19.51.50-2.500.75––Free machining
X2CrMoTi29-41.45920.0251.001.000.0300.01028.0-30.03.50-4.50–0.045Ti: 4×(C+N)+0.15-0.80Superferritic

5. Martensitic and Precipitation Hardening Stainless Steels | Corrosion Resistant Steels

Steel NameSteel NumberC range %Si max %Mn max %P max %S max %Cr range %Mo range %Ni range %N max %V %Others
X15Cr131.40240.12-0.171.001.000.0400.01512.0-14.0––––410
X20Cr131.40210.16-0.251.001.500.0400.01512.0-14.0––––420
X30Cr131.40280.26-0.361.001.500.0400.01512.0-14.0––––420
X29CrS131.40290.25-0.321.001.500.0400.15-0.2512.0-13.50.60–––Free machining
X39Cr131.40310.36-0.421.001.000.0400.01512.5-14.5––––420
X46Cr131.40340.43-0.501.001.000.0400.01512.5-14.5––––420
X46CrS131.40350.43-0.501.002.000.0400.15-0.3512.5-14.0––––Free machining
X65Cr131.40370.58-0.701.001.000.0400.01512.5-14.5––see note–440A, N content specified
X34CrN161.40600.29-0.381.001.000.0400.01515.0-16.5––0.13-0.22–C+N≥0.45, Cr+16N-5C≥16.2
X17CrNi16-21.40570.12-0.221.001.500.0400.01515.0-17.0–1.50-2.50––431
X38CrMo141.44190.36-0.421.001.000.0400.01513.0-14.50.60-1.00––––
X55CrMo141.41100.48-0.601.001.000.0400.01513.0-15.00.50-0.80––0.15–
X3CrNiMo13-41.43130.050.701.500.0400.01512.0-14.00.30-0.703.5-4.5≥0.020–Supermartensitic
X1CrNiMoCu12-5-21.44220.0200.502.000.0400.00311.0-13.01.30-1.804.0-5.00.020–Cu: 0.20-0.80
X50CrMoV151.41160.35-0.551.001.000.0400.01514.0-15.50.50-0.80–see note0.10-0.20440C
X70CrMo151.41090.60-0.750.701.000.0400.01514.0-16.00.40-0.80––––
X2CrNiMoV13-5-21.44150.0300.500.500.0400.01511.5-13.51.50-2.504.5-6.5–0.10-0.50Ti: 0.010, Supermartensitic
X1CrNiMoCu12-7-31.44230.0200.502.000.0400.00311.0-13.02.30-2.806.0-7.00.020–Cu: 0.20-0.80
X53CrSiMoVN16-21.41500.45-0.601.30-1.700.800.0300.01015.0-16.50.20-0.400.400.05-0.200.20-0.40–
X4CrNiMo16-5-11.44180.060.701.500.0400.01515.0-17.00.80-1.504.0-6.0≥0.020––
X14CrMoS171.41040.10-0.171.001.500.0400.15-0.3515.5-17.50.20-0.60–––Free machining
X39CrMo17-11.41220.33-0.451.001.500.0400.01515.5-17.50.80-1.301.00–––
X105CrMo171.41250.95-1.201.001.000.0400.01516.0-18.00.40-0.80–––440C
X40CrMoVN16-21.41230.35-0.501.001.000.0400.01514.0-16.01.00-2.500.500.10-0.301.50–
X90CrMoV181.41120.85-0.951.001.000.0400.01517.0-19.00.90-1.30––0.07-0.12440C
X5CrNiCuNb16-41.45420.070.701.500.0400.01515.0-17.00.603.00-5.0––Nb: 5×C-0.45, Cu: 3.00-5.0, 17-4PH
X7CrNiAl17-71.45680.090.701.000.0400.01516.0-18.0–6.5-7.8––Al: 0.70-1.50, 17-7PH
X5CrNiMoCuNb14-51.45940.070.701.000.0400.01513.0-15.01.20-2.005.0-6.0––Nb: 0.15-0.60, Cu: 1.20-2.00
X1CrNiMoAlTi12-9-21.45300.0150.100.100.0100.00511.5-12.51.85-2.158.5-9.50.010–Al: 0.60-0.80, Ti: 0.28-0.37
X1CrNiMoAlTi12-10-21.45960.0150.100.100.0100.00511.5-12.51.85-2.159.2-10.20.020–Al: 0.80-1.10, Ti: 0.28-0.40
X1CrNiMoAlTi12-11-21.46120.0150.100.100.0100.00511.0-12.51.75-2.2510.2-11.30.010–Al: 1.35-1.75, Ti: 0.20-0.50
X5NiCrTiMoVB25-15-21.46060.081.001.00-2.000.0250.01513.0-16.01.00-1.5024.0-27.0–0.10-0.50B: 0.001-0.010, Al: 0.35, Ti: 1.90-2.30, A-286
X75CrMo14-31.41070.70-0.821.000.800.0350.03013.5-14.52.50-3.200.50N≤0.110.25-0.35440C type
X39CrMo17-11.41220.33-0.451.001.500.0400.01515.5-17.50.80-1.301.00–––
X12CrMoWVNbN10-1-11.49010.10-0.140.300.30-0.600.0200.0109.0-10.00.95-1.050.300.03-0.070.18-0.25Nb: 0.04-0.09, W: 1.45-1.75, Grade 92

6. Austenitic Heat Resistant Stainless Steels | Corrosion Resistant Steels

Steel NameSteel NumberC range %Si max %Mn max %P max %S max %Cr range %Mo max %Ni range %N max %Ti/Nb %Others
X10CrNiTi18-101.45410.04-0.121.002.000.0450.01517.0-19.0–9.0-12.0–Ti: 5×C-0.80321
X10CrNiNb18-101.49610.04-0.121.002.000.0450.01517.0-19.0–9.0-12.0–Nb: 10×C-1.00347
X10CrNiSi18-101.48260.05-0.151.00-2.002.000.0450.03017.0-20.00.808.0-11.0–––
X8CrNiNb16-131.48860.04-0.101.002.000.0450.01515.5-17.00.8012.0-14.0–Nb: 10×C-1.00–
X8CrNiTi18-101.49810.04-0.101.002.000.0450.01517.0-19.0–9.0-12.0–Ti: 5×C-0.80–
X12CrNi23-131.48330.08-0.161.502.000.0450.01522.0-24.0–12.0-14.0––309
X15CrNiSi20-121.48280.10-0.201.50-2.502.000.0450.01519.0-21.0–11.0-13.0––309S
X15CrNiSi25-201.48410.10-0.201.50-2.502.000.0450.01524.0-26.0–19.0-22.0––310S
X15CrNiSi25-211.48570.10-0.201.50-2.502.000.0450.01524.0-26.0–20.0-22.0––310S
X10NiCrAlTi32-211.48760.05-0.151.502.000.0450.01519.0-22.0–31.0-34.0–Ti: 0.15-0.60Al: 0.15-0.60
X8NiCrAlTi32-211.49580.05-0.121.002.000.0300.01519.0-22.0–31.0-35.0–Ti: 0.20-0.60Al: 0.20-0.60
X6NiCrSiNCe35-251.48540.04-0.081.00-2.002.000.0300.01523.0-27.0–34.0-37.00.15-0.40–Ce: 0.03-0.08

7. Ferritic Heat Resistant Stainless Steels | Corrosion Resistant Steels

Steel NameSteel NumberC range %Si range %Mn max %P max %S max %Cr range %Mo max %Ni max %N max %Al range %Others
X10CrAlSi181.47420.08-0.150.70-1.401.000.0400.02517.0-19.00.300.30–0.70-1.40Ti: 8×(C+N)-0.80
X10CrAlSi251.47620.08-0.150.70-1.401.000.0400.02523.0-27.00.300.50–0.70-1.40Ti: 8×(C+N)-0.80
X18CrN281.47490.08-0.200.801.000.0400.01527.0-30.0––0.15-0.30––
X6CrAl131.40020.081.001.000.0400.01512.0-14.0–––0.10-0.30405 (also in Table 4)

8. Austenitic Creep Resistant Stainless Steels | Corrosion Resistant Steels

Steel NameSteel NumberC range %Si max %Mn max %P max %S max %Cr range %Mo range %Ni range %N range %Ti/Nb/B %Others
X6CrNiNb18-101.49410.04-0.101.002.000.0450.01517.0-19.0–9.0-12.0–Nb: 10×C-1.00347H
X6CrNiTiB18-101.49430.04-0.101.002.000.0450.01517.0-19.0–9.0-12.0–Ti: 5×C-0.70, B: 0.001-0.005321HB
X6CrNiMoTi17-12-21.49120.04-0.101.002.000.0450.01516.0-18.02.00-2.5011.0-14.0–Ti: 5×C-0.70316Ti
X6CrNiMoNb17-12-21.49880.04-0.101.002.000.0450.01516.0-18.02.00-2.5011.0-14.0–Nb: 10×C-1.00316Nb
X6CrNiMoB17-12-21.49190.04-0.101.002.000.0450.01516.0-18.02.00-2.5010.0-13.0–B: 0.001-0.005316HB
X3CrNiMoBN17-13-31.49100.02-0.060.502.000.0300.01516.0-18.02.25-3.0012.0-14.00.030-0.070B: 0.001-0.010–
X7CrNiMoBNb16-161.49860.04-0.100.502.000.0300.01515.5-17.01.00-1.5016.0-18.0–Nb: 10×C-1.00, B: 0.003-0.009–
X8CrNiMoVNb16-131.49880.05-0.100.502.000.0300.01515.0-17.01.00-1.5013.0-15.0–Nb: 0.90-1.10V: 0.20-0.35
X8CrNiMoNb16-161.49810.04-0.100.502.000.0300.01515.5-17.01.00-1.5016.0-18.0–Nb: 10×C-1.00–
X10CrNiCuNb18-9-31.49610.08-0.141.002.000.0450.01517.0-19.0–9.0-12.0–Nb: 8×C-1.00Cu: 2.50-3.00
X11CrNiMoNbVB15-13-011.49820.08-0.140.502.000.0300.01514.5-16.00.80-1.2012.5-14.0–Nb: 0.80-1.20, B: 0.002-0.008V: 0.15-0.30
X3CrNiMnMoNbN21-9-5-21.49390.02-0.060.504.0-6.00.0300.01520.0-22.01.50-2.508.0-10.00.15-0.30Nb: 0.30-0.60–
X3CrNiMnMoNbN23-17-5-31.49640.02-0.060.504.0-6.00.0300.01522.0-24.02.50-3.0016.0-18.00.15-0.30Nb: 0.40-0.80800H
X10NiCrAlTi32-201.49580.05-0.121.002.000.0300.01519.0-22.0–31.0-35.0–Ti: 0.20-0.60Al: 0.20-0.60, 800HT
X10NiCrAlTiMoV33-161.49810.05-0.120.802.000.0300.01515.0-17.01.00-1.5032.0-35.0–Ti: 1.80-2.40Al: 0.80-1.40, V: 0.10-0.50
X6NiCrTiMoVB25-15-21.49800.04-0.081.001.00-2.000.0250.01514.0-16.01.00-1.5024.0-27.0–Ti: 1.90-2.35, B: 0.001-0.010Al: 0.40, V: 0.10-0.50, A-286
X1NiCrMoCu31-27-41.45630.020.501.500.0250.01026.0-28.03.00-4.030.0-32.0––Cu: 1.00-2.00, Alloy 825
X1NiCrMoCu25-20-51.45390.020.502.000.0300.01519.0-21.04.0-5.024.0-26.0––Cu: 1.20-2.00, 904L

9. Martensitic Creep Resistant Stainless Steels | Corrosion Resistant Steels

Steel NameSteel NumberC range %Si max %Mn range %P max %S max %Cr range %Mo range %Ni max %V range %Nb/W %Others
X20CrMoV11-11.49220.17-0.230.500.30-0.600.0250.01010.0-12.50.90-1.100.30-0.800.25-0.35–Grade 22, P22
X19CrMoNbVN11-11.49130.15-0.220.200.50-1.000.0200.01010.0-11.50.70-1.000.30-0.700.20-0.30Nb: 0.03-0.08N: 0.02-0.08, Grade 23, P23
X12CrMoWVNbN10-1-11.49010.10-0.140.300.30-0.600.0200.0109.0-10.00.95-1.050.300.18-0.25Nb: 0.04-0.09, W: 1.45-1.75N: 0.03-0.07, Grade 92, P92
X10CrWMoVNb9-21.49010.07-0.140.400.30-0.600.0200.0108.50-9.500.30-0.600.15-0.250.15-0.25Nb: 0.04-0.10, W: 1.50-2.00N: 0.01-0.05, Grade 9
X12CrNiMoV12-31.49380.10-0.160.500.50-1.000.0250.01011.0-12.50.80-1.202.00-2.500.25-0.35–Turbine steel
X3CrNiMoBN17-13-31.49100.02-0.060.502.000.0300.01516.0-18.02.25-3.0012.0-14.0–B: 0.001-0.010N: 0.030-0.070 (also in Table 8)

MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treatment, CNC Machined Products Manufacturer in Turkey, Additive Manufacturing and 3D Printing in Turkey, Quality Enginering and Inspection Service in Turkey, Manufacturing Inspection Service in Turkey, Quality Engineering and Supplier Quality Engineering Service in Turkey, Supplier Quality Control and Inspection Service in Turkey, Resident Engineering Services in Turkey