AISI 5160 Oil Quenched & Tempered at 650°C Overview

AISI 5160 tempered 650°C is AISI 5160 low alloy steel (UNS G51600) in the oil quenched & tempered at 650°C condition. This AISI 5160 tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 5160 conditions in our AISI 5160 yield, tensile and hardness comparison. Looking for AISI 5160 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5160 steel parts in-house and inspects them before shipment.

AISI 5160 Oil Quenched & Tempered at 650°C Designation

AISI 5160
ConditionTempered at 650°C & oil quenched
UNS numberG51600
US nameSAE 5160H, SAE 5160, ASTM G51600, ASTM 5160H, ASTM 5160, ~ASTM 5160
JIS (Japanese) nameSUP9M

AISI 5160 Oil Quenched & Tempered at 650°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 5160 Oil Quenched & Tempered at 650°C Composition detail

C (carbon)0.56–0.64%
Cr (chromium)0.7–0.9%
Fe (iron)97–97.8%
Mn (manganese)0.75–1%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 5160 Oil Quenched & Tempered at 650°C Physical properties

Density7.8–7.9g/cm3

AISI 5160 Oil Quenched & Tempered at 650°C Mechanical properties

Young’s modulus205–213GPa
Specific stiffness26.1–27.2MN.m/kg
Yield strength (elastic limit)720–880MPa
Tensile strength805–990MPa
Specific strength91.7–112kN.m/kg
Elongation16–24% strain
Compressive strength720–880MPa
Flexural modulus205–213GPa
Flexural strength (modulus of rupture)720–880MPa
Shear modulus79–83GPa
Bulk modulus158–174GPa
Poisson’s ratio0.285–0.295 
Shape factor31
Hardness – Vickers248–303HV
Elastic stored energy (springs)1250–1840kJ/m3
Fatigue strength at 10^7 cycles367–426MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
320–489MPa

AISI 5160 Oil Quenched & Tempered at 650°C Impact & fracture properties

Fracture toughness45–74MPa.m0.5
Toughness (G)10.2–24.9kJ/m2

AISI 5160 Oil Quenched & Tempered at 650°C Thermal properties

Melting point1380–1490°C
Maximum service temperature587–640°C
Minimum service temperature-68–-43°C
Thermal conductivity41–48W/m.°C
Specific heat capacity440–520J/kg.°C
Thermal expansion coefficient11.5–13µstrain/°C
Thermal shock resistance277–350°C
Thermal distortion resistance3.29–4MW/m
Latent heat of fusion265–280kJ/kg

AISI 5160 Oil Quenched & Tempered at 650°C Electrical properties

Electrical resistivity22–30µohm.cm
Electrical conductivity5.75–7.84%IACS
Galvanic potential-0.5–-0.42V

AISI 5160 Oil Quenched & Tempered at 650°C Magnetic properties

Magnetic typeMagnetic

AISI 5160 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5110–5210m/s
Mechanical loss coefficient (tan delta)4.4e-4–5.6e-4 

AISI 5160 Oil Quenched & Tempered at 650°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed18 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Poor
Carbon equivalency0.825 – 0.987

AISI 5160 Oil Quenched & Tempered at 650°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 5160 Oil Quenched & Tempered at 650°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 5160 Oil Quenched & Tempered at 650°C Standards with similar compositions

Argentina: IRAM 5160 to IAS
Australia: 5160 to AS 1444
Belgium: 55Cr3 to NBN 235-05, 55Cr3 to NBN 253-05
France: 55C3 to AFNOR NF A35-571
Germany: 1.7176 to DIN 17221, 55Cr3 to DIN 17221
Hungary: 60Cr3 to MSZ 2666, 60CrB3 to MSZ 2666
International: 55Cr3 to ISO 683-14, 60Cr3 to ISO 683-14
Italy: 55Cr3 to UNI 3545
Japan: SUP 9 to JIS G4801, SUP 9A to JIS G4801, SUP11A to JIS G4801, SUP9M to JIS G3311
Mexico: 5160 to NMX-B-203-SCFI, 5160 to NMX-B-300, 5160H to NMX-B-268, 5160H to NMX-B-300, 51B60 to NMX-B-203-SCFI, 51B60 to NMX-B-300, 51B60H to NMX-B-268, 51B60H to NMX-B-300
Pan America: 5160 to COPANT 334
Serbia and Montenegro: C.4332
South Korea: SPS 5 to KS D 3701, SPS 5A to KS D 3701, SPS 7 to KS D 3701, SUP 9 M to KS D 3551
Spain: 55Cr3 to UNE 36015, F.1431 to UNE 36015
Sweden: 2253 to SS 142253, 2254 to SS 142254
Turkey: 55Cr3-1 to TS 2288, 55Cr3-1 to TS 7176
UK: 525A58 to BS 970/2, 525A60 to BS 970/2, 525H60 to BS 970/2, 527A60 to BS 970/1, 527A60 to BS 970/5, 527H60 to BS 970/5
USA: 5160, 5160 to ASTM A29/A29M, 5160 to ASTM A331-95, 5160 to ASTM A519, 5160 to ASTM A829/A829M, 5160 to SAE J404, 5160H to ASTM A331-95, 51B60 to ASTM A331-95, 51B60 to ASTM A519, 51B60 to SAE J404, 51B60H to ASTM A331-95, G51600 to ASTM A1031, G51600 to ASTM A506, UNS G51600, UNS G51601, UNS H51600
Tradenames: F 1 KB, KRUPP 55 CR 3, SAARSTAHL 55 CR 3, SHARON 5100 SERIES C, VR-60, XK5160S, ZAPP VC12