AISI 81B45 Oil Quenched & Tempered at 315°C Material Data Sheet

AISI 81B45 Oil Quenched & Tempered at 315°C Material Data Sheet

AISI 81B45 Oil Quenched & Tempered at 315°C Overview

AISI 81B45 tempered 315°C is AISI 81B45 low alloy steel (UNS G81451) in the oil quenched & tempered at 315°C condition. This AISI 81B45 tempered 315°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 81B45 conditions in our AISI 81B45 yield, tensile and hardness comparison. Looking for AISI 81B45 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 81B45 steel parts in-house and inspects them before shipment.

AISI 81B45 Oil Quenched & Tempered at 315°C Designation

AISI 81B45
ConditionTempered at 315°C & oil quenched
UNS numberG81451, ~H81451
US nameASTM A519 81B45, ASTM A304 81B45, ASTM A29 81B45

AISI 81B45 Oil Quenched & Tempered at 315°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 81B45 Oil Quenched & Tempered at 315°C Composition detail

B (boron)5e-4–0.003%
C (carbon)0.42–0.49%
Cr (chromium)0.3–0.6%
Fe (iron)96.8–98.2%
Mn (manganese)0.7–1.05%
Mo (molybdenum)0.08–0.15%
Ni (nickel)0.15–0.45%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 81B45 Oil Quenched & Tempered at 315°C Physical properties

Density7.8–7.9g/cm3

AISI 81B45 Oil Quenched & Tempered at 315°C Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)1410–1730MPa
Tensile strength1590–1950MPa
Specific strength180–220kN.m/kg
Elongation6–10% strain
Compressive strength1410–1730MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)1410–1730MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor15
Hardness – Vickers425–525HV
Elastic stored energy (springs)4850–7190kJ/m3
Fatigue strength at 10^7 cycles590–682MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
516–780MPa

AISI 81B45 Oil Quenched & Tempered at 315°C Impact & fracture properties

Fracture toughness27–52MPa.m0.5
Toughness (G)3.83–12.1kJ/m2

AISI 81B45 Oil Quenched & Tempered at 315°C Thermal properties

Melting point1420–1500°C
Maximum service temperature275–305°C
Minimum service temperature-53–-23°C
Thermal conductivity35–55W/m.°C
Specific heat capacity440–480J/kg.°C
Thermal expansion coefficient11–13.5µstrain/°C
Thermal shock resistance538–717°C
Thermal distortion resistance2.82–4.59MW/m
Latent heat of fusion265–280kJ/kg

AISI 81B45 Oil Quenched & Tempered at 315°C Electrical properties

Electrical resistivity15–30µohm.cm
Electrical conductivity5.75–11.5%IACS
Galvanic potential-0.51–-0.43V

AISI 81B45 Oil Quenched & Tempered at 315°C Magnetic properties

Magnetic typeMagnetic

AISI 81B45 Oil Quenched & Tempered at 315°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)2.2e-4–2.9e-4 

AISI 81B45 Oil Quenched & Tempered at 315°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed9.45 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.623 – 0.845

AISI 81B45 Oil Quenched & Tempered at 315°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 81B45 Oil Quenched & Tempered at 315°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Susceptible

AISI 81B45 Oil Quenched & Tempered at 315°C Standards with similar compositions

Mexico: 81B45 to NMX-B-300, 81B45H to NMX-B-268, 81B45H to NMX-B-300
Pan America: 81B45 to COPANT 514
USA: 81B45, 81B45 to ASTM A29/A29M, 81B45 to ASTM A322-91, 81B45 to ASTM A331-95, 81B45 to ASTM A519, 81B45 to ASTM A752/A752M, 81B45 to SAE J770, 81B45H, 81B45H to ASTM A304, 81B45H to ASTM A331-95, 81B45H to SAE J1268, 9442, 9445, 9447, EX 12, EX 51, EX 52, EX 53, UNS G81451, UNS H81451, UNS K03810