AISI 9255 Oil Quenched & Tempered at 205°C Material Data Sheet
AISI 9255 Oil Quenched & Tempered at 205°C Overview
| AISI 9255 tempered 205°C is AISI 9255 low alloy steel (UNS G92550, EN 55Si7) in the oil quenched & tempered at 205°C condition. This AISI 9255 tempered 205°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 9255 conditions in our AISI 9255 yield, tensile and hardness comparison. Looking for AISI 9255 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 9255 steel parts in-house and inspects them before shipment. |
AISI 9255 Oil Quenched & Tempered at 205°C Designation
| AISI 9255 | |
| Condition | Tempered at 205°C & oil quenched |
| UNS number | G92550 |
| EN name | 55Si7, 56Si7, 251A58 |
| EN number | 1.5026 |
AISI 9255 Oil Quenched & Tempered at 205°C Typical uses
| Laminated springs, coil springs, torsion bars of heavy section |
AISI 9255 Oil Quenched & Tempered at 205°C Composition detail
| C (carbon) | 0.51 | – | 0.59 | % |
| Fe (iron) | 96.2 | – | 97 | % |
| Mn (manganese) | 0.7 | – | 0.95 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 1.8 | – | 2.2 | % |
AISI 9255 Oil Quenched & Tempered at 205°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 9255 Oil Quenched & Tempered at 205°C Mechanical properties
| Young’s modulus | 206 | – | 216 | GPa |
| Specific stiffness | 26.2 | – | 27.5 | MN.m/kg |
| Yield strength (elastic limit) | 1840 | – | 2260 | MPa |
| Tensile strength | 1890 | – | 2320 | MPa |
| Specific strength | 234 | – | 287 | kN.m/kg |
| Elongation | 1 | – | 2 | % strain |
| Compressive strength | 1840 | – | 2260 | MPa |
| Flexural modulus | 206 | – | 216 | GPa |
| Flexural strength (modulus of rupture) | 1840 | – | 2260 | MPa |
| Shear modulus | 79 | – | 85 | GPa |
| Bulk modulus | 159 | – | 176 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 12 | |||
| Hardness – Vickers | 540 | – | 660 | HV |
| Elastic stored energy (springs) | 8090 | – | 12000 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 668 | – | 771 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 585 | – | 880 | MPa |
AISI 9255 Oil Quenched & Tempered at 205°C Impact & fracture properties
| Fracture toughness | 14 | – | 35 | MPa.m0.5 |
| Toughness (G) | 1.07 | – | 5.02 | kJ/m2 |
AISI 9255 Oil Quenched & Tempered at 205°C Thermal properties
| Melting point | 1390 | – | 1500 | °C |
| Maximum service temperature | 165 | – | 195 | °C |
| Minimum service temperature | -43 | – | -18 | °C |
| Thermal conductivity | 46 | – | 51 | W/m.°C |
| Specific heat capacity | 425 | – | 475 | J/kg.°C |
| Thermal expansion coefficient | 11 | – | 13 | µstrain/°C |
| Thermal shock resistance | 708 | – | 921 | °C |
| Thermal distortion resistance | 3.68 | – | 4.46 | MW/m |
| Latent heat of fusion | 265 | – | 280 | kJ/kg |
AISI 9255 Oil Quenched & Tempered at 205°C Electrical properties
| Electrical resistivity | 15 | – | 35 | µohm.cm |
| Electrical conductivity | 4.93 | – | 11.5 | %IACS |
| Galvanic potential | -0.51 | – | -0.43 | V |
AISI 9255 Oil Quenched & Tempered at 205°C Magnetic properties
| Magnetic type | Magnetic |
AISI 9255 Oil Quenched & Tempered at 205°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5120 | – | 5250 | m/s |
| Mechanical loss coefficient (tan delta) | 1.8e-4 | – | 2.3e-4 | |
AISI 9255 Oil Quenched & Tempered at 205°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 7.62 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.627 – 0.748 |
AISI 9255 Oil Quenched & Tempered at 205°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) Notes: Tempering at a low temperature increases hardness and therefore galling resistance. | Excellent |
| Flammability | Non-flammable |
AISI 9255 Oil Quenched & Tempered at 205°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments | Highly susceptible |
AISI 9255 Oil Quenched & Tempered at 205°C Notes
| AISI 9255 Oil Quenched & Tempered at 205°C Other notes |
| A spring steel, used for more highly stressed applications than carbon steels. |
AISI 9255 Oil Quenched & Tempered at 205°C Standards with similar compositions
| Australia: 9255 to AS 1444 |
| Belgium: 55Si7 to NBN 253-05 |
| Germany: 1.0904 to DIN, 1.5026 to DIN 17222, 55Si7 to DIN 17222 |
| Hungary: 55Si7 to MSZ 2666 |
| India: 50Si7 to IS 4072, 50Si7 to IS 8055, 55Si2Mn90 to IS 4368, 55Si2Mo90 to IS 6967, 55Si7 to IS 1570/4, 55Si7 to IS 2507, 55Si7 to IS 3195, 55Si7 to IS 3431, 55Si7 to IS 3885/1, 55Si7 to IS 3885/2, 55Si7 to IS 4072, 55Si7 to IS 8052, 55Si7 to IS 8055, Grade 2 to IS 8051, Grade 3 to IS 9442 |
| Italy: 56SiMn7KU to UNI 2955/3 |
| Mexico: 9255 to NMX-B-203-SCFI, 9255 to NMX-B-300 |
| Pan America: 9255 to COPANT 334, 9255 to COPANT 514 |
| Serbia and Montenegro: C.2133 |
| Spain: 56Si7 to UNE 36015, F.1440 to UNE 36015 |
| Sweden: 2090 to SS 142090 |
| UK: 250A53 to BS 970/1 |
| USA: 9250, 9255, 9255 to ASTM A29/A29M, 9255 to ASTM A519, UNS G92550 |
| Tradenames: 56 SI 7, A-144, A-145, AIREX, ALAIS AES8, AMBO MS 5, B.S.C. SI-MN, BOCHUMER NZF S/O, BOFORS S-145, BOHLER F110, BOHLER SMF, CHATILLON MN SI, DISQUE H, FAGERSTA FB-S4, FAGERSTA S310, FORTUNA GFD5W, HOFORS SM-5, MULTOLE, NASCOLOY O, POMPEY RS 2, POMPEY RS3, ROCHLING RFA, S.M. STEEL, SAARSTAHL 55 SI 7, SAUT-DU-TARN 55.S6, SILICO MANGANESE SPRING WIRE, SUWEFA GFD5W, SUWEFA SJII, TKS 55 SI 7, TOLEDO H-O SILICOMANGANESE, WEFAHUTTE HLSFW, WIKMANS VH-FS |