AISI 6150 Oil Quenched & Tempered at 425°C Material Data Sheet
AISI 6150 Oil Quenched & Tempered at 425°C Overview
| AISI 6150 tempered 425°C is AISI 6150 low alloy steel (UNS G61500, EN 51CrMnV4) in the oil quenched & tempered at 425°C condition. This AISI 6150 tempered 425°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 6150 conditions in our AISI 6150 yield, tensile and hardness comparison. Looking for AISI 6150 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 6150 steel parts in-house and inspects them before shipment. |
AISI 6150 Oil Quenched & Tempered at 425°C Designation
| AISI 6150 | |
| Condition | Tempered at 425°C & oil quenched |
| UNS number | G61500, H61500, K15048, K15047 |
| US name | ASTM A231, ASTM A232, ASTM A646 Grade 14 |
| EN name | 735A50, BS S 204, 51CrMnV4 |
| EN number | 1.8158, 1.8159, 1.2241 |
| ISO name | 51CrV6, 51CrV4 |
AISI 6150 Oil Quenched & Tempered at 425°C Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 6150 Oil Quenched & Tempered at 425°C Composition detail
| C (carbon) | 0.48 | – | 0.53 | % |
| Cr (chromium) | 0.8 | – | 1.1 | % |
| Fe (iron) | 96.9 | – | 97.7 | % |
| Mn (manganese) | 0.7 | – | 0.9 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 0.15 | – | 0.35 | % |
| V (vanadium) | 0.15 | % |
AISI 6150 Oil Quenched & Tempered at 425°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 6150 Oil Quenched & Tempered at 425°C Mechanical properties
| Young’s modulus | 201 | – | 212 | GPa |
| Specific stiffness | 25.6 | – | 27 | MN.m/kg |
| Yield strength (elastic limit) | 1200 | – | 1470 | MPa |
| Tensile strength | 1290 | – | 1590 | MPa |
| Specific strength | 152 | – | 187 | kN.m/kg |
| Elongation | 8 | – | 12 | % strain |
| Compressive strength | 1200 | – | 1470 | MPa |
| Flexural modulus | 201 | – | 212 | GPa |
| Flexural strength (modulus of rupture) | 1200 | – | 1470 | MPa |
| Shear modulus | 77 | – | 83 | GPa |
| Bulk modulus | 155 | – | 173 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 18 | |||
| Hardness – Vickers | 378 | – | 463 | HV |
| Elastic stored energy (springs) | 3490 | – | 5160 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 511 | – | 591 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 446 | – | 677 | MPa |
AISI 6150 Oil Quenched & Tempered at 425°C Impact & fracture properties
| Fracture toughness | 31 | – | 56 | MPa.m0.5 |
| Toughness (G) | 4.98 | – | 14.2 | kJ/m2 |
AISI 6150 Oil Quenched & Tempered at 425°C Thermal properties
| Melting point | 1410 | – | 1500 | °C |
| Maximum service temperature | 385 | – | 415 | °C |
| Minimum service temperature | -58 | – | -28 | °C |
| Thermal conductivity | 35 | – | 55 | W/m.°C |
| Specific heat capacity | 420 | – | 520 | J/kg.°C |
| Thermal expansion coefficient | 11.5 | – | 13 | µstrain/°C |
| Thermal shock resistance | 465 | – | 591 | °C |
| Thermal distortion resistance | 2.84 | – | 4.53 | MW/m |
| Latent heat of fusion | 265 | – | 280 | kJ/kg |
AISI 6150 Oil Quenched & Tempered at 425°C Electrical properties
| Electrical resistivity | 15 | – | 30 | µohm.cm |
| Electrical conductivity | 5.75 | – | 11.5 | %IACS |
| Galvanic potential | -0.5 | – | -0.42 | V |
AISI 6150 Oil Quenched & Tempered at 425°C Magnetic properties
| Magnetic type | Magnetic |
AISI 6150 Oil Quenched & Tempered at 425°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5060 | – | 5200 | m/s |
| Mechanical loss coefficient (tan delta) | 2.7e-4 | – | 3.4e-4 | |
AISI 6150 Oil Quenched & Tempered at 425°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 11.3 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.787 – 0.93 |
AISI 6150 Oil Quenched & Tempered at 425°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Acceptable |
| Flammability | Non-flammable |
AISI 6150 Oil Quenched & Tempered at 425°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments | Susceptible |
AISI 6150 Oil Quenched & Tempered at 425°C Standards with similar compositions
| Australia: 6150 to AS 1444, 6150H to AS 1444 |
| Belgium: 50CrV4 to NBN 253-02, 50CrV4 to NBN 253-05 |
| France: 50CV4 to AFNOR NF A35-552, 50CV4 to AFNOR NF A35-553, 50CV4 to AFNOR NF A35-571 |
| Germany: 1.2241 to DIN 17350, 1.8159 to DIN 1652, 1.8159 to DIN 17221, 1.8159 to DIN EN 10083, 50CrV4 to DIN EN 10083, 51CrMnV4 to DIN 17350 |
| Hungary: 50CV2 to MSZ 4217, 51CrV4 to MSZ 2666, CrV3 to MSZ 61, CrV3E to MSZ 61, CrV3Z to MSZ 6251 |
| India: 50Cr1V23 to IS 4368, 50Cr4V1 to IS 13352, 50Cr4V2 to IS 11185, 50Cr4V2 to IS 2507, 50Cr4V2 to IS 3885/2, 50Cr4V2 to IS 3930, 50Cr4V2 to IS 7494, 50Cr4V2 to IS 8052, 50CrV4 to IS 4072, 50CrV4 to IS 8055, FDCrV-A to IS 4454/2, TDCrV-A to IS 4454/2, VDCrV-A to IS 4454/2 |
| International: 51CrV4 to ISO 683-1, 51CrV4 to ISO 683-14, 51CrV6 to ISO 683-18, FDCrV-A to ISO 8458-3, TDCrV-A to ISO 8458-3, VDCrV-A to ISO 8458-3 |
| Italy: 50CrV4 to UNI 3545, 50CrV4 to UNI 7064, 50CrV4 to UNI 7065, 50CrV4 to UNI 7845, 50CrV4 to UNI 7874, 50CrV4 to UNI 8893, 51CrMnV4KU to UNI 2955/3, 51CrV3KU to UNI 2955 |
| Japan: SWOCV-V to JIS G3561 |
| Mexico: 6150 to NMX-B-203-SCFI, 6150 to NMX-B-300, 6150H to NMX-B-268, 6150H to NMX-B-300 |
| Pan America: 6150 to COPANT 334 |
| Romania: 50VCr11 to STAS 791, 50VCr11CS to STAS 10677, 51VMnCr11 to STAS 791, 51VMnCr11S to STAS 791, 51VMnCr11X to STAS 791, 51VMnCr11XS to STAS 791 |
| Serbia and Montenegro: C.4830 |
| South Korea: SPS 6 to KS D 3701 |
| Spain: 51CrV4 to UNE 36015, F.1430 to UNE 36015 |
| Turkey: 50CrV4-1,8159 to TS 2288 |
| UK: 51CrV4 to BS EN 10083-1, 51CrV4 to BS EN 10250-3, 51CrV4 to BS EN 10277-5, 735A50 to BS 1429, 735A50 to BS 970/1, 735A51 to BS 970/2, 735H51 to BS 970/2 |
| USA: 6145, 6150, 6150 to ASTM A29/A29M, 6150 to ASTM A519, 6150 to ASTM A829/A829M, 6150 to MIL-S-8503, 6150 to SAE J404, A231 to ASTM A231/A231M, A232 to ASTM A232/A232M, G61500 to ASTM A1031, Grade 14 to ASTM A646-95, UNS G61500, UNS H61500, UNS K15047, UNS K15048 |
| Tradenames: 50 CR V 4, A-143, ACENOR MCV, AMBO FAW, ASCOMETAL 50CV4, BERGISCHE 50 CMV, CYCLOPS L2, DIRO-50 CRV 4, FORTUNA TCV4, GDH-L2, JESSOP ET NO. 6, KRUPP WL 1.8154, PLATE PN 24, SAARSTAHL 50 CRV 4, SHARON 6100 SERIES B, TKS 50 CRV 4, VERTOMAR CV50, VL3, VN-50, WEINGARTNER EW 8159, WESTIG 50 CR V 4, WITTEN PCVWL |