AISI 1040 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 1040 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 1040 Oil Quenched & Tempered at 425°C Overview

AISI 1040 oil quenched tempered 425°C is AISI 1040 medium carbon steel (UNS G10400) in the oil quenched & tempered at 425°C condition. This AISI 1040 oil quenched tempered 425°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1040 conditions in our AISI 1040 yield, tensile and hardness comparison. Looking for AISI 1040 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1040 steel parts in-house and inspects them before shipment.

AISI 1040 Oil Quenched & Tempered at 425°C Designation

AISI 1040
ConditionTempered at 425°C & oil quenched
UNS numberG10400
US nameASTM G10420, ASTM 1042, ASTM 1040, ASME G10400, ASME G10390, ASME 1039
EN name~HS40
ISO name~CE40E4
JIS (Japanese) name~STKM16C, ~STKM16A

AISI 1040 Oil Quenched & Tempered at 425°C Typical uses

Heavy duty shafts, axles, crankshafts, couplings, gears (if given a hardening treatment)

AISI 1040 Oil Quenched & Tempered at 425°C Composition detail

C (carbon)0.37–0.44%
Fe (iron)98.6–99%
Mn (manganese)0.6–0.9%
P (phosphorus)0–0.04%
S (sulfur)0–0.05%

AISI 1040 Oil Quenched & Tempered at 425°C Physical properties

Density7.8–7.9g/cm3

AISI 1040 Oil Quenched & Tempered at 425°C Mechanical properties

Young’s modulus208–216GPa
Specific stiffness26.5–27.5MN.m/kg
Yield strength (elastic limit)495–610MPa
Tensile strength680–835MPa
Specific strength63–77.7kN.m/kg
Elongation16–26% strain
Compressive strength495–610MPa
Flexural modulus208–216GPa
Flexural strength (modulus of rupture)495–610MPa
Shear modulus80–85GPa
Bulk modulus161–176GPa
Poisson’s ratio0.285–0.295 
Shape factor45
Hardness – Vickers220–270HV
Elastic stored energy (springs)583–870kJ/m3
Fatigue strength at 10^7 cycles326–378MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
284–434MPa

AISI 1040 Oil Quenched & Tempered at 425°C Impact & fracture properties

Fracture toughness37–61MPa.m0.5
Toughness (G)6.79–16.7kJ/m2

AISI 1040 Oil Quenched & Tempered at 425°C Thermal properties

Melting point1430–1510°C
Maximum service temperature323–350°C
Minimum service temperature-53–-28°C
Thermal conductivity50–54W/m.°C
Specific heat capacity465–505J/kg.°C
Thermal expansion coefficient10.5–12µstrain/°C
Thermal shock resistance204–261°C
Thermal distortion resistance4.29–5MW/m
Latent heat of fusion270–275kJ/kg

AISI 1040 Oil Quenched & Tempered at 425°C Electrical properties

Electrical resistivity16–19µohm.cm
Electrical conductivity9.07–10.8%IACS
Galvanic potential-0.52–-0.44V

AISI 1040 Oil Quenched & Tempered at 425°C Magnetic properties

Magnetic typeMagnetic

AISI 1040 Oil Quenched & Tempered at 425°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5140–5250m/s
Mechanical loss coefficient (tan delta)5.8e-4–7.3e-4 

AISI 1040 Oil Quenched & Tempered at 425°C Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed21.3 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.47 – 0.59

AISI 1040 Oil Quenched & Tempered at 425°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Can be used for gears only if hardened. Aluminum bronze is the most suitable mating material to minimize galling.
Limited use
FlammabilityNon-flammable

AISI 1040 Oil Quenched & Tempered at 425°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Slightly susceptible

AISI 1040 Oil Quenched & Tempered at 425°C Notes

AISI 1040 Oil Quenched & Tempered at 425°C Other notes
Responds to heat treatment and can be flame or induction hardened to 500 HV for gears and for good wear resistance.

AISI 1040 Oil Quenched & Tempered at 425°C Standards with similar compositions

India: 40C8 to IS 1570/2/1, 45C8 to IS 1570/2/1, C40 to IS 1570/2/1, C45 to IS 1570/2/1, IS 6902 to IS 6902
Mexico: 1038 to NMX-B-301, 1039 to NMX-B-301, 1040 to NMX-B-203-SCFI, 1040 to NMX-B-301, 1042 to NMX-B-301, 1043 to NMX-B-301
Pan America: 1038 to COPANT 331, 1038 to COPANT 333, 1039 to COPANT 333, 1040 to COPANT 330, 1040 to COPANT 331, 1040 to COPANT 333
UK: 080M36 to BS 970/1, 080M40 to BS 970/1, 170H41 to BS 970/1
USA: 1038, 1038 to ASTM A29/A29M, 1038 to ASTM A568/A568M, 1038 to SAE J403, 1039, 1039 to ASTM A29/A29M, 1039 to ASTM A568/A568M, 1039 to SAE J403, 1040, 1040 to ASTM A29/A29M, 1040 to ASTM A513, 1040 to ASTM A519, 1040 to ASTM A568/A568M, 1040 to DoD-F-24669/1, 1040 to FED QQ-S-635B, 1040 to SAE J403, 1042, 1042 to ASTM A29/A29M, 1042 to ASTM A568/A568M, 1042 to SAE J403, 1043, 1043 to ASTM A29/A29M, 1043 to ASTM A568/A568M, 1043 to SAE J403, 1544, C1042 to FED QQ-S-635B, C4 to MIL-S-16788A, CS1040 to MIL-S-11310E, G10380 to ASTM A510/A510M, G10380 to ASTM A576-90b, G10390 to ASTM A510/A510M, G10390 to ASTM A576-90b, G10400 to ASTM A510/A510M, G10400 to ASTM A576-90b, G10420 to ASTM A510/A510M, G10420 to ASTM A576-90b, G10430 to ASTM A510/A510M, G10430 to ASTM A576-90b, UNS G10380, UNS G10380 to UNS, UNS G10390, UNS G10390 to UNS, UNS G10400, UNS G10400 to UNS, UNS G10420, UNS G10420 to UNS, UNS G10430, UNS G10430 to UNS
Tradenames: ALLENOY 1038, ASCOMETAL XC38H1-H2, B/43, BOFORS N91, BOHLER V943, DODGE D-4, DONEGAL D-3, DYNAMIC C-1-4, DYNAMIC C-1-5, FORTUNA W3, GREDE 37, HECLA 37, JESSOP A-5, JESSOP STEEL A-5 (S M-40), KRUPP 1730, RED DIAMOND 9S, S/39, SODING WM, SWB-40M4, TULIPE EXTRA NO. 7, UGINE B 38, V4