AISI 1060 Oil Quenched & Tempered at 205°C Material Data Sheet
AISI 1060 Oil Quenched & Tempered at 205°C Overview
| AISI 1060 oil quenched tempered 205°C is AISI 1060 medium carbon steel (UNS G10600) in the oil quenched & tempered at 205°C condition. This AISI 1060 oil quenched tempered 205°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1060 conditions in our AISI 1060 yield, tensile and hardness comparison. Looking for AISI 1060 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1060 steel parts in-house and inspects them before shipment. |
AISI 1060 Oil Quenched & Tempered at 205°C Designation
| AISI 1060 | |
| Condition | Tempered at 205°C & oil quenched |
| UNS number | G10600 |
| US name | ASTM Class B, ASTM 1060, ASME G10600, ~ASME G10590, ~ASME 1059 |
| EN name | ~HS60 |
AISI 1060 Oil Quenched & Tempered at 205°C Typical uses
| General construction, general mechanical engineering, automotive, tools, axles, gears, springs. |
AISI 1060 Oil Quenched & Tempered at 205°C Composition detail
| C (carbon) | 0.55 | – | 0.65 | % |
| Fe (iron) | 98.4 | – | 98.8 | % |
| Mn (manganese) | 0.6 | – | 0.9 | % |
| P (phosphorus) | 0 | – | 0.04 | % |
| S (sulfur) | 0 | – | 0.05 | % |
AISI 1060 Oil Quenched & Tempered at 205°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 1060 Oil Quenched & Tempered at 205°C Mechanical properties
| Young’s modulus | 208 | – | 216 | GPa |
| Specific stiffness | 26.5 | – | 27.5 | MN.m/kg |
| Yield strength (elastic limit) | 700 | – | 860 | MPa |
| Tensile strength | 990 | – | 1220 | MPa |
| Specific strength | 89.2 | – | 110 | kN.m/kg |
| Elongation | 10 | – | 16 | % strain |
| Compressive strength | 700 | – | 860 | MPa |
| Flexural modulus | 208 | – | 216 | GPa |
| Flexural strength (modulus of rupture) | 700 | – | 860 | MPa |
| Shear modulus | 80 | – | 85 | GPa |
| Bulk modulus | 161 | – | 176 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 33 | |||
| Hardness – Vickers | 290 | – | 360 | HV |
| Elastic stored energy (springs) | 1170 | – | 1730 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 425 | – | 491 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 371 | – | 563 | MPa |
AISI 1060 Oil Quenched & Tempered at 205°C Impact & fracture properties
| Fracture toughness | 33 | – | 57 | MPa.m0.5 |
| Toughness (G) | 5.45 | – | 14.5 | kJ/m2 |
AISI 1060 Oil Quenched & Tempered at 205°C Thermal properties
| Melting point | 1380 | – | 1490 | °C |
| Maximum service temperature | 165 | – | 195 | °C |
| Minimum service temperature | -38 | – | -8 | °C |
| Thermal conductivity | 48 | – | 53 | W/m.°C |
| Specific heat capacity | 480 | – | 520 | J/kg.°C |
| Thermal expansion coefficient | 10 | – | 12 | µstrain/°C |
| Thermal shock resistance | 292 | – | 383 | °C |
| Thermal distortion resistance | 4.16 | – | 5.1 | MW/m |
| Latent heat of fusion | 270 | – | 275 | kJ/kg |
AISI 1060 Oil Quenched & Tempered at 205°C Electrical properties
| Electrical resistivity | 17 | – | 20 | µohm.cm |
| Electrical conductivity | 8.62 | – | 10.1 | %IACS |
| Galvanic potential | -0.51 | – | -0.43 | V |
AISI 1060 Oil Quenched & Tempered at 205°C Magnetic properties
| Magnetic type | Magnetic |
AISI 1060 Oil Quenched & Tempered at 205°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5140 | – | 5250 | m/s |
| Mechanical loss coefficient (tan delta) | 4.1e-4 | – | 5.1e-4 | |
AISI 1060 Oil Quenched & Tempered at 205°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Acceptable |
| Metal hot forming | Acceptable |
| Metal press forming | Acceptable |
| Metal deep drawing | Limited use |
| Machining speed | 14.9 m/min |
| Weldability Notes: Preheating and post weld heat treatments may be required | Good |
| Carbon equivalency | 0.65 – 0.8 |
AISI 1060 Oil Quenched & Tempered at 205°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) Notes: Aluminum bronze is the most suitable mating material to minimize galling. | Acceptable |
| Flammability | Non-flammable |
AISI 1060 Oil Quenched & Tempered at 205°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia | Slightly susceptible |
AISI 1060 Oil Quenched & Tempered at 205°C Standards with similar compositions
| Belgium: C55-2 to NBN 253-02, C55-3 to NBN 253-02 |
| India: 2.49 mm to IS 4824, 60C6 to IS 1570/2/1, 65C6 to IS 1570/2/1, C65 to IS 1570/2/1, IS 4824 to IS 4824 |
| Mexico: 1059 to NMX-B-301, 1060 to NMX-B-301, 1064 to NMX-B-301, 1065 to NMX-B-301, 1561 to NMX-B-301, B366 to NMX-B-366 |
| Pan America: 1060 to COPANT 330, 1060 to COPANT 331, 1060 to COPANT 333, 1061 to COPANT 333 |
| USA: 1055, 1055 to ASTM A568/A568M, 1055 to SAE J403, 1059, 1059 to ASTM A29/A29M, 1059 to ASTM A713, 1059 to SAE J1249, 1060, 1060 to ASTM A29/A29M, 1060 to ASTM A513, 1060 to ASTM A568/A568M, 1060 to ASTM A713, 1060 to DoD-F-24669/1, 1060 to FED QQ-S-00640, 1060 to FED QQ-S-633A, 1060 to MIL-S-16974E, 1060 to SAE J403, 1062, 1064, 1064 to ASTM A29/A29M, 1064 to ASTM A568/A568M, 1064 to ASTM A713, 1064 to SAE J1249, 1065, 1065 to ASTM A29/A29M, 1065 to ASTM A568/A568M, 1065 to ASTM A713, 1065 to SAE J403, 1561, 1561 to ASTM A29/A29M, 1561 to ASTM A713, 7240 to AMS 7240, C6 to MIL-S-16788A, G10590 to ASTM A510/A510M, G10600 to ASTM A510/A510M, G10600 to ASTM A576-90b, G10640 to ASTM A510/A510M, G10650 to ASTM A510/A510M, G15610 to ASTM A510/A510M, G15610 to ASTM A576-90b, Type A Class I to ASTM A417-93, Type A Class II to ASTM A417-93, Type A to ASTM A407-93, Type B Class I to ASTM A417-93, Type B Class II to ASTM A417-93, Type B to ASTM A407-93, Type C Class I to ASTM A417-93, Type C to ASTM A407-93, Type D to ASTM A407-93, Type E to ASTM A407-93, Type F to ASTM A407-93, Type G to ASTM A407-93, Type H to ASTM A407-93, UNS G10590, UNS G10600, UNS G10640, UNS G10640 to UNS, UNS G10650, UNS G10650 to UNS, UNS G15610, UNS K06201 |
| Tradenames: AGATHON BIT STEEL, AMALOY, B/70, DIE BLOCK (A), FORTUNA GSB63, FORTUNA W63, HI-QUA-LED 10L60, INGERSOLL I-60, KRUPP 1740, MARREL M2, PREMIER MB SPRING, PREMIER SPRING, S/70, SHOCK RESISTING, SIMONDS 1064 RULE DIE, SPRING STEEL SHEET, TULIPE EXTRA NO. 5, VEW Z988 |