AISI 5046 Oil Quenched & Tempered at 205°C Material Data Sheet
AISI 5046 Oil Quenched & Tempered at 205°C Material Data Sheet
AISI 5046 Oil Quenched & Tempered at 205°C Overview
AISI 5046 tempered 205°C is AISI 5046 low alloy steel (UNS G50460) in the oil quenched & tempered at 205°C condition. This AISI 5046 tempered 205°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 5046 conditions in our AISI 5046 yield, tensile and hardness comparison. Looking for AISI 5046 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5046 steel parts in-house and inspects them before shipment.
AISI 5046 Oil Quenched & Tempered at 205°C Designation
AISI 5046 Oil Quenched & Tempered at 205°C Thermal properties
Melting point
1420
–
1500
°C
Maximum service temperature
165
–
195
°C
Minimum service temperature
-53
–
-23
°C
Thermal conductivity
40
–
50
W/m.°C
Specific heat capacity
440
–
520
J/kg.°C
Thermal expansion coefficient
11
–
13
µstrain/°C
Thermal shock resistance
497
–
647
°C
Thermal distortion resistance
3.26
–
4.29
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 5046 Oil Quenched & Tempered at 205°C Electrical properties
Electrical resistivity
15
–
30
µohm.cm
Electrical conductivity
5.75
–
11.5
%IACS
Galvanic potential
-0.51
–
-0.43
V
AISI 5046 Oil Quenched & Tempered at 205°C Magnetic properties
Magnetic type
Magnetic
AISI 5046 Oil Quenched & Tempered at 205°C Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5060
–
5200
m/s
Mechanical loss coefficient (tan delta)
2.4e-4
–
3e-4
AISI 5046 Oil Quenched & Tempered at 205°C Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
9.45 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency
0.595 – 0.737
AISI 5046 Oil Quenched & Tempered at 205°C Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 5046 Oil Quenched & Tempered at 205°C Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Susceptible
AISI 5046 Oil Quenched & Tempered at 205°C Standards with similar compositions
Belgium: 46Cr2 to NBN 251
France: 42C2 to AFNOR NF A35-557
Hungary: MC to MSZ 1745
India: 50C6 to IS 14698
Italy: C40 to UNI 6923
Mexico: 5046 to NMX-B-300, 5046H to NMX-B-268, 5046H to NMX-B-300, 50B44 to NMX-B-300, 50B44H to NMX-B-268, 50B44H to NMX-B-300, 50B46 to NMX-B-300, 50B46H to NMX-B-268, 50B46H to NMX-B-300
Pan America: 5046 to COPANT 514
Russia: OsV to GOST 4728
USA: 5046, 5046 to ASTM A29/A29M, 5046 to ASTM A519, 5046 to SAE J770, 50B44 to ASTM A331-95, 50B44 to ASTM A519, 50B46 to ASTM A29/A29M, 50B46 to ASTM A331-95, 50B46 to ASTM A519, 50B46 to ASTM A752/A752M, G50460 to ASTM A1031, Grade 2 to ASTM A983/A983M, UNS G50460, UNS H50460