AISI 8650 Oil Quenched & Tempered at 205°C Material Data Sheet

AISI 8650 Oil Quenched & Tempered at 205°C Material Data Sheet

AISI 8650 Oil Quenched & Tempered at 205°C Overview

AISI 8650 tempered 205°C is AISI 8650 low alloy steel (UNS G86500) in the oil quenched & tempered at 205°C condition. This AISI 8650 tempered 205°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 8650 conditions in our AISI 8650 yield, tensile and hardness comparison. Looking for AISI 8650 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8650 steel parts in-house and inspects them before shipment.

AISI 8650 Oil Quenched & Tempered at 205°C Designation

AISI 8650
ConditionTempered at 205°C & oil quenched
UNS numberG86500
US nameSAE NV5, SAE 8650, SAE 8645H, SAE 8645, ASTM G87400, ASTM G86450, ASTM G86420, ASTM 8650H, ASTM 8650, ASTM 8645H, ASTM 8645, ~SAE G86450, ~ASTM G86500, ~ASTM 8645
JIS (Japanese) nameSFNCM 1030 D

AISI 8650 Oil Quenched & Tempered at 205°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 8650 Oil Quenched & Tempered at 205°C Composition detail

C (carbon)0.48–0.53%
Cr (chromium)0.4–0.6%
Fe (iron)96.5–97.7%
Mn (manganese)0.75–1%
Mo (molybdenum)0.15–0.25%
Ni (nickel)0.4–0.7%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 8650 Oil Quenched & Tempered at 205°C Physical properties

Density7.8–7.9g/cm3

AISI 8650 Oil Quenched & Tempered at 205°C Mechanical properties

Young’s modulus206–216GPa
Specific stiffness26.2–27.5MN.m/kg
Yield strength (elastic limit)1500–1850MPa
Tensile strength1740–2140MPa
Specific strength190–235kN.m/kg
Elongation8–12% strain
Compressive strength1500–1850MPa
Flexural modulus206–216GPa
Flexural strength (modulus of rupture)1500–1850MPa
Shear modulus79–85GPa
Bulk modulus159–176GPa
Poisson’s ratio0.285–0.295 
Shape factor14
Hardness – Vickers470–580HV
Elastic stored energy (springs)5350–8000kJ/m3
Fatigue strength at 10^7 cycles630–728MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
551–833MPa

AISI 8650 Oil Quenched & Tempered at 205°C Impact & fracture properties

Fracture toughness25–51MPa.m0.5
Toughness (G)3.26–11.2kJ/m2

AISI 8650 Oil Quenched & Tempered at 205°C Thermal properties

Melting point1410–1500°C
Maximum service temperature165–195°C
Minimum service temperature-48–-18°C
Thermal conductivity35–45W/m.°C
Specific heat capacity460–500J/kg.°C
Thermal expansion coefficient11–12.5µstrain/°C
Thermal shock resistance594–760°C
Thermal distortion resistance2.94–3.89MW/m
Latent heat of fusion265–280kJ/kg

AISI 8650 Oil Quenched & Tempered at 205°C Electrical properties

Electrical resistivity23–35µohm.cm
Electrical conductivity4.93–7.5%IACS
Galvanic potential-0.5–-0.42V

AISI 8650 Oil Quenched & Tempered at 205°C Magnetic properties

Magnetic typeMagnetic

AISI 8650 Oil Quenched & Tempered at 205°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5120–5250m/s
Mechanical loss coefficient (tan delta)2.1e-4–2.7e-4 

AISI 8650 Oil Quenched & Tempered at 205°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed8.23 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.742 – 0.913

AISI 8650 Oil Quenched & Tempered at 205°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 8650 Oil Quenched & Tempered at 205°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Susceptible

AISI 8650 Oil Quenched & Tempered at 205°C Standards with similar compositions

Mexico: 8650 to NMX-B-203-SCFI, 8650 to NMX-B-300, 8650H to NMX-B-268, 8650H to NMX-B-300, 8655 to NMX-B-203-SCFI, 8655 to NMX-B-300, 8655H to NMX-B-268, 8655H to NMX-B-300
Pan America: 8650 to COPANT 334, 8650 to COPANT 514
USA: 8650, 8650 to ASTM A29/A29M, 8650 to ASTM A322-91, 8650 to ASTM A331-95, 8650 to ASTM A519, 8650 to SAE J770, 8650H, 8650H to ASTM A304, 8650H to ASTM A331-95, 8650H to SAE J1268, 8653, 8655, 8655 to ASTM A29/A29M, 8655 to ASTM A322-91, 8655 to ASTM A331-95, 8655 to ASTM A519, 8655 to ASTM A752/A752M, 8655 to ASTM A829/A829M, 8655 to SAE J404, 8655 to SAE J770, 8655H, 8655H to ASTM A304, 8655H to ASTM A331-95, 8655H to SAE J1268, 8750, G86500 to ASTM A1031, G86550 to ASTM A1031, UNS G86500, UNS G86550, UNS H86500, UNS H86550, UNS K13550
Tradenames: SHARON 8600 SERIES B, VB-50