AISI 1060 Oil Quenched & Tempered at 650°C Material Data Sheet

AISI 1060 Oil Quenched & Tempered at 650°C Material Data Sheet

AISI 1060 Oil Quenched & Tempered at 650°C Overview

AISI 1060 oil quenched tempered 650°C is AISI 1060 medium carbon steel (UNS G10600) in the oil quenched & tempered at 650°C condition. This AISI 1060 oil quenched tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1060 conditions in our AISI 1060 yield, tensile and hardness comparison. Looking for AISI 1060 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1060 steel parts in-house and inspects them before shipment.

AISI 1060 Oil Quenched & Tempered at 650°C Designation

AISI 1060
ConditionTempered at 650°C & oil quenched
UNS numberG10600
US nameASTM Class B, ASTM 1060, ASME G10600, ~ASME G10590, ~ASME 1059
EN name~HS60

AISI 1060 Oil Quenched & Tempered at 650°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 1060 Oil Quenched & Tempered at 650°C Composition detail

C (carbon)0.55–0.65%
Fe (iron)98.4–98.8%
Mn (manganese)0.6–0.9%
P (phosphorus)0–0.04%
S (sulfur)0–0.05%

AISI 1060 Oil Quenched & Tempered at 650°C Physical properties

Density7.8–7.9g/cm3

AISI 1060 Oil Quenched & Tempered at 650°C Mechanical properties

Young’s modulus208–216GPa
Specific stiffness26.5–27.5MN.m/kg
Yield strength (elastic limit)465–580MPa
Tensile strength720–880MPa
Specific strength59.2–73.9kN.m/kg
Elongation18–28% strain
Compressive strength465–580MPa
Flexural modulus208–216GPa
Flexural strength (modulus of rupture)465–580MPa
Shear modulus80–85GPa
Bulk modulus161–176GPa
Poisson’s ratio0.285–0.295 
Shape factor47
Hardness – Vickers210–260HV
Elastic stored energy (springs)515–785kJ/m3
Fatigue strength at 10^7 cycles340–392MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
297–449MPa

AISI 1060 Oil Quenched & Tempered at 650°C Impact & fracture properties

Fracture toughness42–70MPa.m0.5
Toughness (G)8.77–21.9kJ/m2

AISI 1060 Oil Quenched & Tempered at 650°C Thermal properties

Melting point1380–1490°C
Maximum service temperature305–345°C
Minimum service temperature-53–-23°C
Thermal conductivity48–53W/m.°C
Specific heat capacity480–520J/kg.°C
Thermal expansion coefficient10–12µstrain/°C
Thermal shock resistance194–258°C
Thermal distortion resistance4.16–5.1MW/m
Latent heat of fusion270–275kJ/kg

AISI 1060 Oil Quenched & Tempered at 650°C Electrical properties

Electrical resistivity17–20µohm.cm
Electrical conductivity8.62–10.1%IACS
Galvanic potential-0.51–-0.43V

AISI 1060 Oil Quenched & Tempered at 650°C Magnetic properties

Magnetic typeMagnetic

AISI 1060 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5140–5250m/s
Mechanical loss coefficient (tan delta)5.8e-4–7.3e-4 

AISI 1060 Oil Quenched & Tempered at 650°C Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed21.3 m/min
Weldability
Notes: Preheating and post weld heat treatments may be required
Good
Carbon equivalency0.65 – 0.8

AISI 1060 Oil Quenched & Tempered at 650°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 1060 Oil Quenched & Tempered at 650°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Slightly susceptible

AISI 1060 Oil Quenched & Tempered at 650°C Standards with similar compositions

Belgium: C55-2 to NBN 253-02, C55-3 to NBN 253-02
India: 2.49 mm to IS 4824, 60C6 to IS 1570/2/1, 65C6 to IS 1570/2/1, C65 to IS 1570/2/1, IS 4824 to IS 4824
Mexico: 1059 to NMX-B-301, 1060 to NMX-B-301, 1064 to NMX-B-301, 1065 to NMX-B-301, 1561 to NMX-B-301, B366 to NMX-B-366
Pan America: 1060 to COPANT 330, 1060 to COPANT 331, 1060 to COPANT 333, 1061 to COPANT 333
USA: 1055, 1055 to ASTM A568/A568M, 1055 to SAE J403, 1059, 1059 to ASTM A29/A29M, 1059 to ASTM A713, 1059 to SAE J1249, 1060, 1060 to ASTM A29/A29M, 1060 to ASTM A513, 1060 to ASTM A568/A568M, 1060 to ASTM A713, 1060 to DoD-F-24669/1, 1060 to FED QQ-S-00640, 1060 to FED QQ-S-633A, 1060 to MIL-S-16974E, 1060 to SAE J403, 1062, 1064, 1064 to ASTM A29/A29M, 1064 to ASTM A568/A568M, 1064 to ASTM A713, 1064 to SAE J1249, 1065, 1065 to ASTM A29/A29M, 1065 to ASTM A568/A568M, 1065 to ASTM A713, 1065 to SAE J403, 1561, 1561 to ASTM A29/A29M, 1561 to ASTM A713, 7240 to AMS 7240, C6 to MIL-S-16788A, G10590 to ASTM A510/A510M, G10600 to ASTM A510/A510M, G10600 to ASTM A576-90b, G10640 to ASTM A510/A510M, G10650 to ASTM A510/A510M, G15610 to ASTM A510/A510M, G15610 to ASTM A576-90b, Type A Class I to ASTM A417-93, Type A Class II to ASTM A417-93, Type A to ASTM A407-93, Type B Class I to ASTM A417-93, Type B Class II to ASTM A417-93, Type B to ASTM A407-93, Type C Class I to ASTM A417-93, Type C to ASTM A407-93, Type D to ASTM A407-93, Type E to ASTM A407-93, Type F to ASTM A407-93, Type G to ASTM A407-93, Type H to ASTM A407-93, UNS G10590, UNS G10600, UNS G10640, UNS G10640 to UNS, UNS G10650, UNS G10650 to UNS, UNS G15610, UNS K06201
Tradenames: AGATHON BIT STEEL, AMALOY, B/70, DIE BLOCK (A), FORTUNA GSB63, FORTUNA W63, HI-QUA-LED 10L60, INGERSOLL I-60, KRUPP 1740, MARREL M2, PREMIER MB SPRING, PREMIER SPRING, S/70, SHOCK RESISTING, SIMONDS 1064 RULE DIE, SPRING STEEL SHEET, TULIPE EXTRA NO. 5, VEW Z988