How do the AISI 1141 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1141 resulfurized medium carbon steel (UNS G11410) side by side for 8 conditions: annealed, as rolled, normalized, oil quenched & tempered at 205°C, oil quenched & tempered at 315°C, oil quenched & tempered at 425°C, oil quenched & tempered at 540°C, oil quenched & tempered at 650°C. All values are taken from the individual AISI 1141 material data sheets linked below.
AISI 1141 Yield, Tensile and Hardness by Condition
| Condition | Yield strength (MPa) | Tensile strength (MPa) | Hardness (HV) | Elongation (%) | Machining speed (m/min) |
|---|---|---|---|---|---|
| Annealed | 315–390 | 540–660 | 150–190 | 20–31 | 36.6 |
| As Rolled | 320–395 | 595–745 | 180–220 | 17–27 | 30.5 |
| Normalized | 365–445 | 645–780 | 188–228 | 18–28 | 29.9 |
| Oil Quenched & Tempered at 205°C | 1090–1340 | 1470–1800 | 415–505 | 4–8 | 12.5 |
| Oil Quenched & Tempered at 315°C | 1150–1420 | 1230–1520 | 375–455 | 7–11 | 14.3 |
| Oil Quenched & Tempered at 425°C | 925–1140 | 1050–1290 | 300–370 | 9–15 | 17.7 |
| Oil Quenched & Tempered at 540°C | 685–845 | 805–990 | 240–290 | 14–22 | 23.2 |
| Oil Quenched & Tempered at 650°C | 530–655 | 640–780 | 200–245 | 18–28 | 28.7 |
AISI 1141 Differences Compared with Annealed
The table below shows how much each AISI 1141 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.
| Condition | Yield strength | Tensile strength | Hardness | Elongation |
|---|---|---|---|---|
| As Rolled | +1% | +12% | +18% | -14% |
| Normalized | +15% | +19% | +22% | -10% |
| Oil Quenched & Tempered at 205°C | +245% | +172% | +171% | -76% |
| Oil Quenched & Tempered at 315°C | +265% | +129% | +144% | -65% |
| Oil Quenched & Tempered at 425°C | +193% | +95% | +97% | -53% |
| Oil Quenched & Tempered at 540°C | +117% | +50% | +56% | -29% |
| Oil Quenched & Tempered at 650°C | +68% | +18% | +31% | -10% |
AISI 1141 Strength and Hardness Charts
AISI 1141 Heat Treatment Key Points
The highest tensile strength of AISI 1141 in these data sheets is reached in the oil quenched & tempered at 205°C condition (1470–1800 MPa). The softest condition is annealed (150–190 HV), with a machining speed of 36.6 m/min, which is usually preferred for machining and forming. For oil quenched AISI 1141, raising the tempering temperature from 205°C to 650°C lowers hardness from 415–505 HV to 200–245 HV, trading strength for toughness and ductility.
AISI 1141 is a resulfurized free-machining grade. See how it compares with the other free-machining steels in our resulfurized steels comparison.
AISI 1141 Material Data Sheets
AISI 1141 Annealed | AISI 1141 As Rolled | AISI 1141 Normalized | AISI 1141 Oil Quenched & Tempered at 205°C | AISI 1141 Oil Quenched & Tempered at 315°C | AISI 1141 Oil Quenched & Tempered at 425°C | AISI 1141 Oil Quenched & Tempered at 540°C | AISI 1141 Oil Quenched & Tempered at 650°C | All AISI 1141 conditions
Looking for AISI 1141 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1141 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.