AISI 205 Stainless Steel, Annealed, Mechanical Properties

AISI 205 Stainless Steel, Annealed, Mechanical Properties

Young’s modulus193–201GPa
Specific stiffness24.7–25.9MN.m/kg
Yield strength (elastic limit)425–525MPa
Tensile strength745–925MPa
Specific strength54.5–67.4kN.m/kg
Elongation40–70% strain
Compressive strength425–525MPa
Flexural modulus193–201GPa
Flexural strength (modulus of rupture)425–525MPa
Shear modulus75–80GPa
Bulk modulus136–149GPa
Poisson’s ratio0.265–0.275 
Shape factor47   
Hardness – Vickers195–245HV
Hardness – Rockwell B93–103HRB
Hardness – Rockwell C10–22HRC
Hardness – Brinell190–228HB
Elastic stored energy (springs)1090–1540kJ/m^3
Fatigue strength at 10^7 cycles348–406MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles293–482MPa

AISI 205 Stainless Steel, Annealed, Impact & fracture properties

Fracture toughness96–153MPa.m^0.5
Toughness (G)48.9–114kJ/m^2

AISI 205, wrought
Condition                                                                                                   Solution annealed
UNS number                                                                                                   S20500
US name                                                                                                   ASTM S20500

MODULUS METAL
Sand Casting in Turkey, Permanent Mold Casting in Turkey, Gravity Die Casting in Turkey, Pressure Die Casting in Turkey, High-Pressure Die Casting in Turkey, Investment Casting in Turkey, Foundry in Turkey, Plastic Injection Molding in Turkey, Press Bending ( Press Brake) Products in Turkey, Laser and Plasma Cutting in Turkey, Welded Construction in Turkey, Heat Treated, CNC Machined Products Manufacturer in Turkey, Additive Manufacturing and 3D Printing in Turkey, Quality Enginering and Inspection Service in Turkey, Manufacturing Inspection Service in Turkey, Quality Engineering and Supplier Quality Engineering Service in Turkey, Supplier Quality Control and Inspection Service in Turkey, Resident Engineering Services in Turkey