AISI 1144 Annealed vs As Rolled vs Normalized vs Oil Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 1144 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength, hardness, elongation and machining speed of AISI 1144 resulfurized medium carbon steel (UNS G11440) side by side for 8 conditions: annealed, as rolled, normalized, oil quenched & tempered at 205°C, oil quenched & tempered at 315°C, oil quenched & tempered at 425°C, oil quenched & tempered at 540°C, oil quenched & tempered at 650°C. All values are taken from the individual AISI 1144 material data sheets linked below.

AISI 1144 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)Machining speed (m/min)
Annealed310–385525–645155–19020–3045.7
As Rolled375–470630–775195–24016–2636.6
Normalized360–440600–740180–22516–2636.6
Oil Quenched & Tempered at 205°C560–695780–970255–30513–2127.1
Oil Quenched & Tempered at 315°C555–690775–965240–29013–2128
Oil Quenched & Tempered at 425°C545–680760–935230–28014–2229.3
Oil Quenched & Tempered at 540°C510–635725–890215–26516–2430.5
Oil Quenched & Tempered at 650°C450–555645–800200–24518–2833.5

AISI 1144 Differences Compared with Annealed

The table below shows how much each AISI 1144 condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength, hardness or elongation.

ConditionYield strengthTensile strengthHardnessElongation
As Rolled+22%+20%+26%-16%
Normalized+15%+15%+17%-16%
Oil Quenched & Tempered at 205°C+81%+50%+62%-32%
Oil Quenched & Tempered at 315°C+79%+49%+54%-32%
Oil Quenched & Tempered at 425°C+76%+45%+48%-28%
Oil Quenched & Tempered at 540°C+65%+38%+39%-20%
Oil Quenched & Tempered at 650°C+45%+24%+29%-8%

AISI 1144 Strength and Hardness Charts

AISI 1144 Yield strength by condition (MPa)Annealed310–385As Rolled375–470Normalized360–440OQ&T 205°C560–695OQ&T 315°C555–690OQ&T 425°C545–680OQ&T 540°C510–635OQ&T 650°C450–555
AISI 1144 Tensile strength by condition (MPa)Annealed525–645As Rolled630–775Normalized600–740OQ&T 205°C780–970OQ&T 315°C775–965OQ&T 425°C760–935OQ&T 540°C725–890OQ&T 650°C645–800
AISI 1144 Hardness by condition (HV)Annealed155–190As Rolled195–240Normalized180–225OQ&T 205°C255–305OQ&T 315°C240–290OQ&T 425°C230–280OQ&T 540°C215–265OQ&T 650°C200–245

AISI 1144 Heat Treatment Key Points

The highest tensile strength of AISI 1144 in these data sheets is reached in the oil quenched & tempered at 205°C condition (780–970 MPa). The softest condition is annealed (155–190 HV), with a machining speed of 45.7 m/min, which is usually preferred for machining and forming. For oil quenched AISI 1144, raising the tempering temperature from 205°C to 650°C lowers hardness from 255–305 HV to 200–245 HV, trading strength for toughness and ductility.

AISI 1144 is a resulfurized free-machining grade. See how it compares with the other free-machining steels in our resulfurized steels comparison.

AISI 1144 Material Data Sheets

AISI 1144 Annealed | AISI 1144 As Rolled | AISI 1144 Normalized | AISI 1144 Oil Quenched & Tempered at 205°C | AISI 1144 Oil Quenched & Tempered at 315°C | AISI 1144 Oil Quenched & Tempered at 425°C | AISI 1144 Oil Quenched & Tempered at 540°C | AISI 1144 Oil Quenched & Tempered at 650°C | All AISI 1144 conditions

Looking for AISI 1144 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1144 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.