AISI 50B60 Oil Quenched & Tempered at 650°C Material Data Sheet

AISI 50B60 Oil Quenched & Tempered at 650°C Material Data Sheet

AISI 50B60 Oil Quenched & Tempered at 650°C Overview

AISI 50B60 tempered 650°C is AISI 50B60 low alloy steel (UNS G50601) in the oil quenched & tempered at 650°C condition. This AISI 50B60 tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 50B60 conditions in our AISI 50B60 yield, tensile and hardness comparison. Looking for AISI 50B60 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 50B60 steel parts in-house and inspects them before shipment.

AISI 50B60 Oil Quenched & Tempered at 650°C Designation

AISI 50B60
ConditionTempered at 650°C & oil quenched
UNS numberG50601
US nameASTM 50B60, ~ASTM 51B60, ~ASME 51B60

AISI 50B60 Oil Quenched & Tempered at 650°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 50B60 Oil Quenched & Tempered at 650°C Composition detail

B (boron)5e-4–0.003%
C (carbon)0.55–0.65%
Cr (chromium)0.4–0.6%
Fe (iron)97.3–98.1%
Mn (manganese)0.75–1%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 50B60 Oil Quenched & Tempered at 650°C Physical properties

Density7.8–7.9g/cm3

AISI 50B60 Oil Quenched & Tempered at 650°C Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)700–860MPa
Tensile strength805–990MPa
Specific strength89.2–110kN.m/kg
Elongation15–23% strain
Compressive strength700–860MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)700–860MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor32
Hardness – Vickers260–320HV
Elastic stored energy (springs)1200–1780kJ/m3
Fatigue strength at 10^7 cycles367–426MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
320–489MPa

AISI 50B60 Oil Quenched & Tempered at 650°C Impact & fracture properties

Fracture toughness46–76MPa.m0.5
Toughness (G)10.8–26.6kJ/m2

AISI 50B60 Oil Quenched & Tempered at 650°C Thermal properties

Melting point1380–1490°C
Maximum service temperature587–640°C
Minimum service temperature-68–-43°C
Thermal conductivity40–50W/m.°C
Specific heat capacity440–520J/kg.°C
Thermal expansion coefficient11–13µstrain/°C
Thermal shock resistance275–359°C
Thermal distortion resistance3.26–4.29MW/m
Latent heat of fusion265–280kJ/kg

AISI 50B60 Oil Quenched & Tempered at 650°C Electrical properties

Electrical resistivity15–30µohm.cm
Electrical conductivity5.75–11.5%IACS
Galvanic potential-0.51–-0.43V

AISI 50B60 Oil Quenched & Tempered at 650°C Magnetic properties

Magnetic typeMagnetic

AISI 50B60 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)4.5e-4–5.6e-4 

AISI 50B60 Oil Quenched & Tempered at 650°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed17.4 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Poor
Carbon equivalency0.755 – 0.937

AISI 50B60 Oil Quenched & Tempered at 650°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 50B60 Oil Quenched & Tempered at 650°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 50B60 Oil Quenched & Tempered at 650°C Standards with similar compositions

Czech Republic: 14160 to CSN 414160
France: 55C2 to AFNOR
Germany: 1.7138 to DIN, 52MnCrB3 to DIN
Mexico: 50B60 to NMX-B-300, 50B60H to NMX-B-268, 50B60H to NMX-B-300
Pan America: 50B60 to COPANT 514
USA: 5060, 50B50, 50B50 to ASTM A229/A229M, 50B50 to SAE J770, 50B60, 50B60 to ASTM A29/A29M, 50B60 to ASTM A322-91, 50B60 to ASTM A331-95, 50B60 to ASTM A519, 50B60 to ASTM A752/A752M, 50B60 to SAE J770, 50B60H, 50B60H to ASTM A304, 50B60H to ASTM A331-95, 50B60H to SAE J1268, EX 3, UNS G50501, UNS G50600, UNS G50601, UNS H50501, UNS H50601
Tradenames: ABRADUR C 65 K, DICROME, FIRTH-BROWN CR2T, FIRTH-BROWN CR3T, FIRTH-BROWN DICROME, KRUPP 2007, KRUPP 52 MNCRB 3, KRUPP 65 CR 3, VICKERS B.C.T.