AISI 81B45 Oil Quenched & Tempered at 650°C Material Data Sheet
AISI 81B45 Oil Quenched & Tempered at 650°C Material Data Sheet
AISI 81B45 Oil Quenched & Tempered at 650°C Overview
AISI 81B45 tempered 650°C is AISI 81B45 low alloy steel (UNS G81451) in the oil quenched & tempered at 650°C condition. This AISI 81B45 tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 81B45 conditions in our AISI 81B45 yield, tensile and hardness comparison. Looking for AISI 81B45 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 81B45 steel parts in-house and inspects them before shipment.
AISI 81B45 Oil Quenched & Tempered at 650°C Designation
AISI 81B45
Condition
Tempered at 650°C & oil quenched
UNS number
G81451, ~H81451
US name
ASTM A519 81B45, ASTM A304 81B45, ASTM A29 81B45
AISI 81B45 Oil Quenched & Tempered at 650°C Typical uses
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 81B45 Oil Quenched & Tempered at 650°C Composition detail
B (boron)
5e-4
–
0.003
%
C (carbon)
0.42
–
0.49
%
Cr (chromium)
0.3
–
0.6
%
Fe (iron)
96.8
–
98.2
%
Mn (manganese)
0.7
–
1.05
%
Mo (molybdenum)
0.08
–
0.15
%
Ni (nickel)
0.15
–
0.45
%
P (phosphorus)
0
–
0.035
%
S (sulfur)
0
–
0.04
%
Si (silicon)
0.15
–
0.35
%
AISI 81B45 Oil Quenched & Tempered at 650°C Physical properties
Density
7.8
–
7.9
g/cm3
AISI 81B45 Oil Quenched & Tempered at 650°C Mechanical properties
Young’s modulus
201
–
212
GPa
Specific stiffness
25.6
–
27
MN.m/kg
Yield strength (elastic limit)
710
–
875
MPa
Tensile strength
805
–
990
MPa
Specific strength
90.4
–
111
kN.m/kg
Elongation
16
–
24
% strain
Compressive strength
710
–
875
MPa
Flexural modulus
201
–
212
GPa
Flexural strength (modulus of rupture)
710
–
875
MPa
Shear modulus
77
–
83
GPa
Bulk modulus
155
–
173
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
31
Hardness – Vickers
255
–
315
HV
Elastic stored energy (springs)
1230
–
1840
kJ/m3
Fatigue strength at 10^7 cycles
367
–
426
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
AISI 81B45 Oil Quenched & Tempered at 650°C Thermal properties
Melting point
1420
–
1500
°C
Maximum service temperature
607
–
640
°C
Minimum service temperature
-68
–
-43
°C
Thermal conductivity
35
–
55
W/m.°C
Specific heat capacity
440
–
480
J/kg.°C
Thermal expansion coefficient
11
–
13.5
µstrain/°C
Thermal shock resistance
271
–
362
°C
Thermal distortion resistance
2.82
–
4.59
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 81B45 Oil Quenched & Tempered at 650°C Electrical properties
Electrical resistivity
15
–
30
µohm.cm
Electrical conductivity
5.75
–
11.5
%IACS
Galvanic potential
-0.51
–
-0.43
V
AISI 81B45 Oil Quenched & Tempered at 650°C Magnetic properties
Magnetic type
Magnetic
AISI 81B45 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5060
–
5200
m/s
Mechanical loss coefficient (tan delta)
4.5e-4
–
5.6e-4
AISI 81B45 Oil Quenched & Tempered at 650°C Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
17.4 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency
0.623 – 0.845
AISI 81B45 Oil Quenched & Tempered at 650°C Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 81B45 Oil Quenched & Tempered at 650°C Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible
AISI 81B45 Oil Quenched & Tempered at 650°C Standards with similar compositions
Mexico: 81B45 to NMX-B-300, 81B45H to NMX-B-268, 81B45H to NMX-B-300
Pan America: 81B45 to COPANT 514
USA: 81B45, 81B45 to ASTM A29/A29M, 81B45 to ASTM A322-91, 81B45 to ASTM A331-95, 81B45 to ASTM A519, 81B45 to ASTM A752/A752M, 81B45 to SAE J770, 81B45H, 81B45H to ASTM A304, 81B45H to ASTM A331-95, 81B45H to SAE J1268, 9442, 9445, 9447, EX 12, EX 51, EX 52, EX 53, UNS G81451, UNS H81451, UNS K03810