AISI 1141 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 1141 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 1141 Oil Quenched & Tempered at 425°C Overview

AISI 1141 oil quenched tempered 425°C is AISI 1141 resulfurized medium carbon steel (UNS G11410) in the oil quenched & tempered at 425°C condition. This AISI 1141 oil quenched tempered 425°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 1141 conditions in our AISI 1141 yield, tensile and hardness comparison. See also the resulfurized free-machining steels comparison. Looking for AISI 1141 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 1141 steel parts in-house and inspects them before shipment.

AISI 1141 Oil Quenched & Tempered at 425°C Designation

AISI 1141
ConditionTempered at 425°C & oil quenched
UNS numberG11410
US nameASTM G11410, ASTM 1141 Class B, ASTM 1141 Class A, ASTM 1141

AISI 1141 Oil Quenched & Tempered at 425°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 1141 Oil Quenched & Tempered at 425°C Composition detail

C (carbon)0.37–0.45%
Fe (iron)97.7–98.2%
Mn (manganese)1.35–1.65%
P (phosphorus)0–0.04%
S (sulfur)0.08–0.13%

AISI 1141 Oil Quenched & Tempered at 425°C Physical properties

Density7.8–7.9g/cm3

AISI 1141 Oil Quenched & Tempered at 425°C Mechanical properties

Young’s modulus200–215GPa
Specific stiffness25.5–27.4MN.m/kg
Yield strength (elastic limit)925–1140MPa
Tensile strength1050–1290MPa
Specific strength118–145kN.m/kg
Elongation9–15% strain
Compressive strength925–1140MPa
Flexural modulus200–215GPa
Flexural strength (modulus of rupture)925–1140MPa
Shear modulus77–84GPa
Bulk modulus155–175GPa
Poisson’s ratio0.285–0.295 
Shape factor23
Hardness – Vickers300–370HV
Elastic stored energy (springs)2080–3110kJ/m3
Fatigue strength at 10^7 cycles441–511MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
385–586MPa

AISI 1141 Oil Quenched & Tempered at 425°C Impact & fracture properties

Fracture toughness22–40MPa.m0.5
Toughness (G)2.5–7.2kJ/m2

AISI 1141 Oil Quenched & Tempered at 425°C Thermal properties

Melting point1430–1510°C
Maximum service temperature322–350°C
Minimum service temperature-38–-8°C
Thermal conductivity48–53W/m.°C
Specific heat capacity440–480J/kg.°C
Thermal expansion coefficient12–13.5µstrain/°C
Thermal shock resistance344–440°C
Thermal distortion resistance3.67–4.28MW/m
Latent heat of fusion270–275kJ/kg

AISI 1141 Oil Quenched & Tempered at 425°C Electrical properties

Electrical resistivity16–19µohm.cm
Electrical conductivity9.07–10.8%IACS
Galvanic potential-0.52–-0.44V

AISI 1141 Oil Quenched & Tempered at 425°C Magnetic properties

Magnetic typeMagnetic

AISI 1141 Oil Quenched & Tempered at 425°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5050–5240m/s
Mechanical loss coefficient (tan delta)3.4e-4–4.3e-4 

AISI 1141 Oil Quenched & Tempered at 425°C Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed17.7 m/min
Weldability
Notes: Preheating and post weld heat treatments may be required
Poor
Carbon equivalency0.595 – 0.725

AISI 1141 Oil Quenched & Tempered at 425°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Aluminum bronze is the most suitable mating material to minimize galling.
Acceptable
FlammabilityNon-flammable

AISI 1141 Oil Quenched & Tempered at 425°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; Other susceptible environments: Nitrate, hydroxide, carbonate, ammonia
Slightly susceptible

AISI 1141 Oil Quenched & Tempered at 425°C Standards with similar compositions

Argentina: IRAM 1141 to IAS
India: 40C15S12 to IS 1570/3, 40C15S12 to IS 9175/13, 40Mn15S12 to IS 3930, 40Mn2S12 to IS 1570/3
Italy: 40SMnPb10 to UNI 4838
Japan: SUM42 to JIS G4804
Mexico: 1139 to NMX-B-301, 1141 to NMX-B-301
Pan America: 1041 to COPANT 333, 1141 to COPANT 330, 1141 to COPANT 331, 1141 to COPANT 332, 1141 to COPANT 514
USA: 1139, 1139 to ASTM A29/A29M, 1139 to SAE J1249, 1141, 1141 Class A to ASTM A311/A311M, 1141 Class B to ASTM A311/A311M, 1141 to ASTM A29/A29M, 1141 to ASTM A519, 1141 to FED QQ-S-633A, 1141 to FED QQ-S-637A, 1141 to SAE J403, C1139 to FED QQ-S-637A, G11390 to ASTM A510/A510M, G11390 to ASTM A576-90b, G11410 to ASTM A510/A510M, G11410 to ASTM A576-90b, UNS G11390, UNS G11410
Tradenames: AMERCUT C-1141, BETHLEHEM 33C, JALCASE 8, RY-AX, S-1141, STRAIN TEMPERED 1141