AISI 4130 or AISI 4140? This AISI 4130 vs AISI 4140 comparison puts the two grades side by side using only the values in our AISI 4130 and AISI 4140 material data sheets: chemical composition, yield strength, tensile strength, hardness, elongation, fracture toughness, fatigue strength and machining speed, condition by condition. Differences are calculated from the mid-point of each range and show AISI 4140 relative to AISI 4130.
Note on the heat treatment data: in these data sheets the AISI 4130 quenched and tempered values are for water quenching, while the AISI 4140 values are for oil quenching, and the AISI 4130 normalized data sheet is for air melted material. The rows are matched by tempering temperature, so read the quenched and tempered differences with the quench medium in mind.
AISI 4130 vs AISI 4140 Chemical Composition
| Element (%) | AISI 4130 | AISI 4140 |
|---|---|---|
| C | 0.28–0.33 | 0.38–0.43 |
| Mn | 0.4–0.6 | 0.75–1 |
| Si | 0.15–0.35 | 0.15–0.35 |
| Cr | 0.8–1.1 | 0.8–1.1 |
| Mo | 0.15–0.25 | 0.15–0.25 |
| Ni | — | — |
| P | 0–0.035 | 0–0.035 |
| S | 0–0.04 | 0–0.04 |
AISI 4130 vs AISI 4140 Yield strength
| Condition | AISI 4130 (MPa) | AISI 4140 (MPa) | AISI 4140 vs AISI 4130 |
|---|---|---|---|
| Annealed | 320–400 | 370–460 | +15% |
| Normalized | 483–534 | 595–715 | +29% |
| Q&T 205°C | 1320–1610 | 1480–1810 | +12% |
| Q&T 315°C | 1240–1520 | 1290–1580 | +4% |
| Q&T 425°C | 1070–1320 | 1020–1260 | -5% |
| Q&T 540°C | 820–1000 | 750–920 | -8% |
| Q&T 650°C | 630–775 | 595–715 | -7% |
AISI 4130 AISI 4140. Dark bar = minimum, light bar = maximum of the range.
AISI 4130 vs AISI 4140 Tensile strength
| Condition | AISI 4130 (MPa) | AISI 4140 (MPa) | AISI 4140 vs AISI 4130 |
|---|---|---|---|
| Annealed | 500–620 | 595–720 | +17% |
| Normalized | 621–686 | 915–1130 | +56% |
| Q&T 205°C | 1450–1770 | 1600–1950 | +10% |
| Q&T 315°C | 1350–1650 | 1400–1710 | +4% |
| Q&T 425°C | 1150–1410 | 1120–1380 | -2% |
| Q&T 540°C | 925–1140 | 855–1050 | -8% |
| Q&T 650°C | 730–895 | 680–840 | -6% |
AISI 4130 vs AISI 4140 Hardness
| Condition | AISI 4130 (HV) | AISI 4140 (HV) | AISI 4140 vs AISI 4130 |
|---|---|---|---|
| Annealed | 145–185 | 183–223 | +23% |
| Normalized | 183–223 | 275–335 | +50% |
| Q&T 205°C | 420–515 | 455–565 | +9% |
| Q&T 315°C | 390–480 | 400–490 | +2% |
| Q&T 425°C | 345–420 | 335–410 | -3% |
| Q&T 540°C | 285–355 | 260–320 | -9% |
| Q&T 650°C | 225–275 | 210–260 | -6% |
AISI 4130 vs AISI 4140 Elongation
| Condition | AISI 4130 (%) | AISI 4140 (%) | AISI 4140 vs AISI 4130 |
|---|---|---|---|
| Annealed | 22–34 | 20–31 | -9% |
| Normalized | 5–18 | 13.5–21.5 | +52% |
| Q&T 205°C | 8–12 | 6–10 | -20% |
| Q&T 315°C | 8.5–13.5 | 7–11 | -18% |
| Q&T 425°C | 10–16 | 10–16 | +0% |
| Q&T 540°C | 13–21 | 14–22 | +6% |
| Q&T 650°C | 17–27 | 17–27 | +0% |
AISI 4130 vs AISI 4140 Fracture toughness
| Condition | AISI 4130 (MPa·m0.5) | AISI 4140 (MPa·m0.5) | AISI 4140 vs AISI 4130 |
|---|---|---|---|
| Annealed | 75–122 | 76–120 | -1% |
| Normalized | 72–114 | 68–107 | -6% |
| Q&T 205°C | 29–53 | 24–48 | -12% |
| Q&T 315°C | 30–55 | 29–54 | -2% |
| Q&T 425°C | 34–60 | 36–63 | +5% |
| Q&T 540°C | 43–71 | 45–74 | +4% |
| Q&T 650°C | 48–79 | 50–80 | +2% |
AISI 4130 vs AISI 4140 Fatigue strength at 107 cycles
| Condition | AISI 4130 (MPa) | AISI 4140 (MPa) | AISI 4140 vs AISI 4130 |
|---|---|---|---|
| Annealed | 263–307 | 297–341 | +12% |
| Normalized | 299–347 | 402–465 | +34% |
| Q&T 205°C | 555–639 | 593–684 | +7% |
| Q&T 315°C | 526–608 | 540–622 | +2% |
| Q&T 425°C | 472–545 | 463–535 | -2% |
| Q&T 540°C | 405–470 | 383–442 | -6% |
| Q&T 650°C | 343–397 | 326–379 | -5% |
AISI 4130 vs AISI 4140 Machining speed
| Condition | AISI 4130 (m/min) | AISI 4140 (m/min) | AISI 4140 vs AISI 4130 |
|---|---|---|---|
| Annealed | 29.9 | 25 | -16% |
| Normalized | 24.4 | 15.8 | -35% |
| Q&T 205°C | 9.75 | 8.84 | -9% |
| Q&T 315°C | 10.4 | 10.4 | +0% |
| Q&T 425°C | 12.2 | 12.8 | +5% |
| Q&T 540°C | 14.9 | 16.8 | +13% |
| Q&T 650°C | 19.2 | 21.3 | +11% |
AISI 4130 vs AISI 4140 Weldability, Processing and Corrosion
| Property | AISI 4130 | AISI 4140 |
|---|---|---|
| Weldability | Good | Good |
| Carbon equivalency | 0.537–0.7 | 0.695–0.867 |
AISI 4130 vs AISI 4140: Key Differences
On average across 7 matched conditions, AISI 4140 has 10% higher tensile strength than AISI 4130. On average across 7 matched conditions, AISI 4140 has 6% higher yield strength than AISI 4130. Fracture toughness is practically the same for AISI 4130 and AISI 4140 (average difference -1% across 7 matched conditions). On average across 7 matched conditions, AISI 4140 has 5% lower machining speed than AISI 4130. Elongation is practically the same for AISI 4130 and AISI 4140 (average difference +2% across 7 matched conditions).
AISI 4130 vs 4140 FAQ
Yes. Across 7 matched conditions in our data sheets, AISI 4140 has on average about 10% higher tensile strength and 6% higher yield strength than AISI 4130. Note that our 4130 quenched and tempered data is for water quenching and the 4140 data for oil quenching.
The main difference is carbon: AISI 4130 contains 0.28–0.33% carbon and AISI 4140 0.38–0.43%. Chromium (0.8–1.1%) and molybdenum (0.15–0.25%) are the same in both data sheets.
Annealed AISI 4130 has a machining speed of 29.9 m/min and annealed AISI 4140 25 m/min in our data sheets, so 4130 machines faster.
Annealed AISI 4130 is 145–185 HV and annealed AISI 4140 is 183–223 HV in our data sheets.
Fracture toughness is practically the same on average across the matched conditions in our data (difference -1%). Annealed: 75–122 MPa·m^0.5 for 4130 vs 76–120 for 4140.
AISI 4130 and AISI 4140 Material Data Sheets
AISI 4130 Annealed | AISI 4130 Air Melted, Normalized | AISI 4130 Water Quenched & Tempered at 205°C | AISI 4130 Water Quenched & Tempered at 315°C | AISI 4130 Water Quenched & Tempered at 425°C | AISI 4130 Water Quenched & Tempered at 540°C | AISI 4130 Water Quenched & Tempered at 650°C | All AISI 4130 conditions
AISI 4140 Annealed | AISI 4140 Normalized | AISI 4140 Oil Quenched & Tempered at 205°C | AISI 4140 Oil Quenched & Tempered at 315°C | AISI 4140 Oil Quenched & Tempered at 425°C | AISI 4140 Oil Quenched & Tempered at 540°C | AISI 4140 Oil Quenched & Tempered at 650°C | All AISI 4140 conditions
Need AISI 4130 or AISI 4140 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.