Home » Brass Alloys » CuZn36Pb3 (C36000) Free-Cutting Brass, Soft Material Data Sheet
CuZn36Pb3 (C36000) Free-Cutting Brass, Soft Material Data Sheet
CuZn36Pb3 (C36000) Free-Cutting Brass Material Data Sheet (Wrought, Soft)
CuZn36Pb3 C36000 Soft Overview
CuZn36Pb3 C36000 soft is a wrought brass (UNS C36000), known as free-cutting brass. Condition: Soft. This CuZn36Pb3 C36000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn36Pb3 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn36Pb3 brass parts in-house and inspects them before shipment.
CuZn36Pb3 Designation
CuZn36Pb3, wrought
Condition
Soft
UNS number
C36000
EN name
CW603N
ISO name
CuZn36Pb3
JIS (Japanese) name
C3600
CuZn36Pb3 Typical uses
Machined parts on automatic lathes, bushes, bearings, screws, extrusions.
CuZn36Pb3 C36000 Soft Composition detail
Cu (copper)
58.4
–
64.5
%
Fe (iron)
0
–
0.35
%
Pb (lead)
2.5
–
3.7
%
Zn (zinc)
33
–
37.5
%
CuZn36Pb3 Physical properties
Density
8.18
–
8.35
g/cm3
CuZn36Pb3 C36000 Soft Mechanical properties
Young’s modulus
98.9
–
105
GPa
Specific stiffness
11.9
–
12.7
MN.m/kg
Yield strength (elastic limit)
150
–
160
MPa
Tensile strength
360
–
400
MPa
Specific strength
18.1
–
19.4
kN.m/kg
Elongation
36
–
40
% strain
Compressive strength
150
–
160
MPa
Flexural modulus
98.9
–
105
GPa
Flexural strength (modulus of rupture)
150
–
160
MPa
Shear modulus
36.6
–
38.9
GPa
Bulk modulus
107
–
113
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
29
Hardness – Vickers
75
–
80
HV
Elastic stored energy (springs)
110
–
126
kJ/m3
Fatigue strength at 10^7 cycles
165
–
177
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
153
–
191
MPa
CuZn36Pb3 Impact & fracture properties
Fracture toughness
61.3
–
63.3
MPa.m0.5
Toughness (G)
36.5
–
39.8
kJ/m2
CuZn36Pb3 C36000 Soft Thermal properties
Melting point
877
–
897
°C
Maximum service temperature
97
–
110
°C
Minimum service temperature
-273
°C
Thermal conductivity
120
–
125
W/m.°C
Specific heat capacity
376
–
378
J/kg.°C
Thermal expansion coefficient
19.4
–
20.6
µstrain/°C
Thermal shock resistance
72.1
–
80.2
°C
Thermal distortion resistance
5.91
–
6.35
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn36Pb3 Electrical properties
Electrical resistivity
6.5
–
6.8
µohm.cm
Electrical conductivity
25.4
–
26.5
%IACS
Galvanic potential
-0.34
–
-0.26
V
CuZn36Pb3 Magnetic properties
Magnetic type
Non-magnetic
CuZn36Pb3 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3460
–
3570
m/s
Mechanical loss coefficient (tan delta)
1.56e-4
–
1.78e-4
CuZn36Pb3 Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
104 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor
CuZn36Pb3 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear) Notes: Contains lead which lubricates, improving resistance.
Excellent
Flammability
Non-flammable
CuZn36Pb3 C36000 Soft Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn36Pb3 Notes
CuZn36Pb3 C36000 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn36Pb3 Standards with similar compositions
Australia: 360 to AS 1567, C36000 to AS 2738
Canada: HC.5.ZP353(360) to CSA
Finland: CuZn36Pb3 to SFS 2922
France: CuZn36Pb3 to NF A51-105
International: CuZn36Pb3 to ISO 1637, CuZn36Pb3 to ISO 426-2
UK: CZ124 to BS 2874
USA: 61.5Cu-35.5Zn-3Pb to QQ B-613, 61.5Cu-35.5Zn-3Pb to QQ B-626, 61.5Cu-35Zn-3.1Pb to AMS 4610, C36000, C36000 to ASTM B16/B16M, C36000 to SAE J463, UNS C36000