Home » Brass Alloys » CuZn33 (C26800) Yellow Brass, Soft Material Data Sheet
CuZn33 (C26800) Yellow Brass, Soft Material Data Sheet
CuZn33 (C26800) Yellow Brass Material Data Sheet (Wrought, Soft)
CuZn33 C26800 Soft Overview
CuZn33 C26800 soft is a wrought brass (UNS C26800), known as yellow brass. Condition: Soft. This CuZn33 C26800 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn33 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn33 brass parts in-house and inspects them before shipment.
CuZn33 Designation
CuZn33, wrought
Condition
Soft
UNS number
C26800
EN name
CW506L
ISO name
CuZn33
JIS (Japanese) name
C2680
CuZn33 C26800 Soft Composition detail
Cu (copper)
63.8
–
68.7
%
Fe (iron)
0
–
0.05
%
Pb (lead)
0
–
0.15
%
Zn (zinc)
31.3
–
36
%
CuZn33 Physical properties
Density
8.38
–
8.55
g/cm3
CuZn33 C26800 Soft Mechanical properties
Young’s modulus
99.9
–
106
GPa
Specific stiffness
11.8
–
12.5
MN.m/kg
Yield strength (elastic limit)
120
–
130
MPa
Tensile strength
325
–
340
MPa
Specific strength
14.2
–
15.4
kN.m/kg
Elongation
56
–
58
% strain
Compressive strength
120
–
130
MPa
Flexural modulus
99.9
–
106
GPa
Flexural strength (modulus of rupture)
120
–
130
MPa
Shear modulus
37
–
39.2
GPa
Bulk modulus
108
–
115
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
29
Hardness – Vickers
64
–
75
HV
Elastic stored energy (springs)
69.7
–
82.4
kJ/m3
Fatigue strength at 10^7 cycles
155
–
159
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
150
–
165
MPa
CuZn33 Impact & fracture properties
Fracture toughness
67.9
–
70.4
MPa.m0.5
Toughness (G)
44.4
–
48.6
kJ/m2
CuZn33 C26800 Soft Thermal properties
Melting point
927
–
942
°C
Maximum service temperature
200
–
210
°C
Minimum service temperature
-273
°C
Thermal conductivity
118
–
124
W/m.°C
Specific heat capacity
378
–
380
J/kg.°C
Thermal expansion coefficient
18.9
–
20.1
µstrain/°C
Thermal shock resistance
58.8
–
66
°C
Thermal distortion resistance
5.97
–
6.45
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn33 Electrical properties
Electrical resistivity
6.17
–
6.61
µohm.cm
Electrical conductivity
26.1
–
27.9
%IACS
Galvanic potential
-0.32
–
-0.24
V
CuZn33 Magnetic properties
Magnetic type
Non-magnetic
CuZn33 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3430
–
3540
m/s
Mechanical loss coefficient (tan delta)
2.37e-4
–
2.78e-4
CuZn33 Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Excellent
Metal press forming
Acceptable
Metal deep drawing
Acceptable
Machining speed
57.9 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor
CuZn33 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn33 C26800 Soft Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn33 Notes
CuZn33 C26800 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn33 Standards with similar compositions
Australia: C26800 to AS 2738, C27000 to AS 2738
Canada: HC.4.Z34(268) to CSA HC.4.2
France: CuZn33 to NF A51-101, CuZn33 to NF A51-104
International: CuZn33 to ISO 1634, CuZn33 to ISO 1638, CuZn33 to ISO 426-1
Japan: C2680 P/R to JIS H3100, C2680 TW to JIS H3320, C2700 BD to JIS H3250, C2700 BE to JIS H3250, C2700 T to JIS H3300, C2700 W to JIS H3260
UK: CZ107 to BS 2870, CZ107 to BS 2873
USA: 65.5Cu-35.5Zn to AMS 4555, 65Cu-35Zn to QQ B-613, 65Cu-35Zn to QQ W-321, C26800, C26800 to ASTM B36/B36M, C26800 to ASTM B587, C26800 to SAE J463, C27000, C27000 to AMS 4712E, C27000 to ASTM B134, C27000 to ASTM B135M, C27000 to ASTM B587, C27000 to SAE J463, UNS C26800, UNS C27000