CuZn38Sn1 C46400 hard is a wrought brass (UNS C46400), known as naval brass. Condition: Hard. This CuZn38Sn1 C46400 hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn38Sn1 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn38Sn1 brass parts in-house and inspects them before shipment.

CuZn38Sn1 Designation

CuZn38Sn1, wrought
ConditionHard
UNS numberC46400
EN nameCW719R
ISO nameCuZn38Sn1
JIS (Japanese) nameC4640 / C4641

CuZn38Sn1 Typical uses

Heat exchangers, marine equipment, underwater items, forged parts.

CuZn38Sn1 C46400 Hard Composition detail

Cu (copper)58.2–62.8%
Fe (iron)0–0.1%
Pb (lead)0–0.2%
Sn (tin)0.5–1%
Zn (zinc)36.7–40.5%

CuZn38Sn1 Physical properties

Density8.189–8.36g/cm3

CuZn38Sn1 C46400 Hard Mechanical properties

Young’s modulus98.9–105GPa
Specific stiffness11.9–12.7MN.m/kg
Yield strength (elastic limit)160–170MPa
Tensile strength390–400MPa
Specific strength19.3–20.6kN.m/kg
Elongation33–35% strain
Compressive strength160–170MPa
Flexural modulus98.9–105GPa
Flexural strength (modulus of rupture)160–170MPa
Shear modulus36.6–38.9GPa
Bulk modulus107–113GPa
Poisson’s ratio0.34–0.35 
Shape factor28
Hardness – Vickers99–121HV
Elastic stored energy (springs)125–143kJ/m3
Fatigue strength at 10^7 cycles174–177MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
171–181MPa

CuZn38Sn1 Impact & fracture properties

Fracture toughness59.4–61.3MPa.m0.5
Toughness (G)34.2–37.3kJ/m2

CuZn38Sn1 C46400 Hard Thermal properties

Melting point902–919°C
Maximum service temperature150–160°C
Minimum service temperature-200  °C
Thermal conductivity120–128W/m.°C
Specific heat capacity376–378J/kg.°C
Thermal expansion coefficient19.4–20.6µstrain/°C
Thermal shock resistance76.9–85.2°C
Thermal distortion resistance5.93–6.48MW/m
Latent heat of fusion220–240kJ/kg

CuZn38Sn1 Electrical properties

Electrical resistivity6.46–6.92µohm.cm
Electrical conductivity24.9–26.7%IACS
Galvanic potential-0.34–-0.26V

CuZn38Sn1 Magnetic properties

Magnetic typeNon-magnetic

CuZn38Sn1 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3450–3570m/s
Mechanical loss coefficient (tan delta)1.38e-4–1.56e-4 

CuZn38Sn1 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed61 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Good

CuZn38Sn1 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn38Sn1 C46400 Hard Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn38Sn1 Notes

CuZn38Sn1 C46400 Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn38Sn1 Standards with similar compositions

Australia: C46400 to AS 2738
Canada: HC.4.ZT381P to CSA HC.4.9, HC.4.ZT391(464) to CSA HC.4.9
Europe: CW719R to CEN EN 12163, CW719R to CEN EN 12165, CW719R to CEN EN 12167, CW719R to CEN EN 12420, CW719R to CEN EN 1653
Japan: C4640 P to JIS H3100, C4641 BD to JIS H3250, C4641 BE to JIS H3250
USA: 464 to QQ B-639B, 60.5Cu-38.7Zn-0.8Sn to AMS 4611, 60.5Cu-38Zn-.8Sn.7Pb to QQ B-626, 60.5Cu-38Zn-.8Sn.7Pb to QQ B-637, 60Cu-37.5Zn1.8Pb.7Sn to QQ B-626, 60Cu-37.5Zn1.8Pb.7Sn to QQ B-637, 60Cu-39.2Zn-.8Sn to ASME SB171, 60Cu-39.2Zn-.8Sn to QQ B-637, C46400, C46400 to ASTM B124M, C46400 to ASTM B171/B171M, C46400 to ASTM B21M, C46400 to ASTM B283, C46400 to SAE J463, UNS C46400
Tradenames: AIRCO NO. 20 BRONZE ROD, BLUE TIP NAVAL BRASS, BOHNALLOY R60N, BRIDGEPORT BRONZE, BRIDGEPORT NO. 24, BRIDGEPORT NO. 45, CERRO N5, CHAMET BRONZE, CHAMET BRONZE, TYPE A, DELTA N5, IMI 365, MCKECHNIE ETS, MUELLER 4640, MUELLER 4643, NAVAL BRASS 24, NAVAL BRASS, UNINHIBITED, NAVAL BRASS-462, NAVAL BRASS-464, NAVAL NO. 6, NORANDA 4640, REVERE ALLOY NO. 385, REVERE ALLOY NO. 464, REVERE ALLOY NO. 464A, REVERE NO. 381, ROMAN BRONZE, SCOVILL ALLOY 464 NAVAL BRASS (A), SCOVILL NAVAL BRASS 464, SEMALLOY NO. 2975, TITAN BRONZE, TITAN NAVAL BRONZE, TITAN NO. 6A, TOBIN BRONZE 4641, WESTERN ALLOY NO. 98