CuZn5 (C21000) Gilding Metal, Soft Material Data Sheet

CuZn5 (C21000) Gilding Metal Material Data Sheet (Wrought, Soft)

CuZn5 C21000 Soft Overview

CuZn5 C21000 soft is a wrought brass (UNS C21000), known as gilding metal. Condition: Soft. This CuZn5 C21000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn5 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn5 brass parts in-house and inspects them before shipment.

CuZn5 Designation

CuZn5, wrought
ConditionSoft
UNS numberC21000
EN nameCW500L
ISO nameCuZn5
GB (Chinese) nameH96
JIS (Japanese) nameC2100

CuZn5 Typical uses

Ammunition caps.

CuZn5 C21000 Soft Composition detail

Cu (copper)93.9–96.1%
Fe (iron)0–0.05%
Pb (lead)0–0.03%
Zn (zinc)3.92–6%

CuZn5 Physical properties

Density8.59–8.76g/cm3

CuZn5 C21000 Soft Mechanical properties

Young’s modulus116–124GPa
Specific stiffness13.4–14.3MN.m/kg
Yield strength (elastic limit)90–100MPa
Tensile strength260–270MPa
Specific strength10.4–11.5kN.m/kg
Elongation43–45% strain
Compressive strength90–100MPa
Flexural modulus116–124GPa
Flexural strength (modulus of rupture)90–100MPa
Shear modulus42.9–45.9GPa
Bulk modulus125–134GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers58–62HV
Elastic stored energy (springs)33.7–41.8kJ/m3
Fatigue strength at 10^7 cycles134–137MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
130–141MPa

CuZn5 Impact & fracture properties

Fracture toughness76–79.2MPa.m0.5
Toughness (G)47.6–52.9kJ/m2

CuZn5 C21000 Soft Thermal properties

Melting point1060–1070°C
Maximum service temperature200–210°C
Minimum service temperature-200  °C
Thermal conductivity230–235W/m.°C
Specific heat capacity381–383J/kg.°C
Thermal expansion coefficient16.5–17.5µstrain/°C
Thermal shock resistance43.5–49.8°C
Thermal distortion resistance13.3–14.1MW/m
Latent heat of fusion220–240kJ/kg

CuZn5 Electrical properties

Electrical resistivity3.02–3.16µohm.cm
Electrical conductivity54.6–57.1%IACS
Galvanic potential-0.22–-0.14V

CuZn5 Magnetic properties

Magnetic typeNon-magnetic

CuZn5 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3650–3780m/s
Mechanical loss coefficient (tan delta)4e-4–4.94e-4 

CuZn5 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingAcceptable
Metal press formingExcellent
Metal deep drawingAcceptable
Machining speed39.6 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good

CuZn5 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn5 C21000 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Susceptible

CuZn5 Notes

CuZn5 C21000 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn5 Standards with similar compositions

Australia: C21000 to AS 2738
Canada: HC.4.Z5(210) to CSA HC.4.2
Europe: CW500L to CEN EN 12163, CW500L to CEN EN 12449, CW500L to CEN EN 1652
France: CuZn5 to NF A51-101
Germany: 2.022 to DIN, CuZn5 to DIN
International: CuZn5 to ISO 1634, CuZn5 to ISO 1638, CuZn5 to ISO 426-1
Japan: C2100 P/R to JIS H3100, C2100 W to JIS H3260
USA: 95Cu-5Zn to MIL C-21768, 95Cu-5Zn to QQ W-321, C21000, C21000 to ASTM B134, C21000 to ASTM B36/B36M, C21000 to ASTM B587, C21000 to CDA Datasheet, C21000 to SAE J463, UNS C21000
Tradenames: 2100, 95/5 GILDING METAL, ANACONDA 210, ANSONIA ALLOY C21000, BRIDGEPORT NO. 26, FUCHS 2195, GILDING, GILDING 95%, GILDING METAL 26, GILDING METAL, 95%, GILDING METAL, SCOVILL ALLOY 110, OLIN GILDING METAL 210, PRYM 221, REVERE GILDING METAL, RIVERSIDE 64, SEYMOUR 2295, VOLCO NO. 95, WESTERN GILDING ALLOY NO. 5, WIELAND-M05