CuZn30Pb2 (C85400) Brass, Sand-Cast Material Data Sheet

CuZn30Pb2 (C85400) Brass Material Data Sheet (Cast, Sand-Cast)

CuZn30Pb2 C85400 Sand-Cast Overview

CuZn30Pb2 C85400 sand-cast is a cast brass (UNS C85400). Condition: Sand-Cast. This CuZn30Pb2 C85400 sand-cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn30Pb2 brass castings from Turkey (Türkiye)? Modulus Metal supplies CuZn30Pb2 brass castings with in-house CNC machining and inspects them before shipment.

CuZn30Pb2 Designation

CuZn30Pb2
UNS numberC85400
ISO nameCuZn33Pb2

CuZn30Pb2 Typical uses

General-purpose castings, plumbing & gas fittings, electrical items, centrifugal castings.

CuZn30Pb2 C85400 Sand-Cast Composition detail

Al (aluminum)0–0.35%
Cu (copper)65–70%
Fe (iron)0–0.7%
Ni (nickel)0–1%
Pb (lead)1.5–3.8%
Si (silicon)0–0.05%
Sn (tin)0.5–1.5%
Zn (zinc)24–32%

CuZn30Pb2 Physical properties

Density8.119–8.28g/cm3

CuZn30Pb2 C85400 Sand-Cast Mechanical properties

Young’s modulus96–98GPa
Specific stiffness11.7–12MN.m/kg
Yield strength (elastic limit)70–110MPa
Tensile strength221–248MPa
Specific strength8.54–13.4kN.m/kg
Elongation11–30% strain
Compressive strength70–110MPa
Flexural modulus96–98GPa
Flexural strength (modulus of rupture)70–110MPa
Shear modulus35.5–36.2GPa
Bulk modulus104–106GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers45–65HV
Elastic stored energy (springs)26.3–59.8kJ/m3
Fatigue strength at 10^7 cycles109–120MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
97.3–134MPa

CuZn30Pb2 Impact & fracture properties

Fracture toughness73.1–86.4MPa.m0.5
Toughness (G)55.4–76.5kJ/m2

CuZn30Pb2 C85400 Sand-Cast Thermal properties

Melting point952–967°C
Maximum service temperature120–130°C
Minimum service temperature-273  °C
Thermal conductivity86.5–90W/m.°C
Specific heat capacity375–377J/kg.°C
Thermal expansion coefficient20.2–21.2µstrain/°C
Thermal shock resistance34.8–54.9°C
Thermal distortion resistance4.13–4.41MW/m
Latent heat of fusion220–240kJ/kg

CuZn30Pb2 Electrical properties

Electrical resistivity8.32–8.91µohm.cm
Electrical conductivity19.4–20.7%IACS
Galvanic potential-0.31–-0.23V

CuZn30Pb2 Magnetic properties

Magnetic typeNon-magnetic

CuZn30Pb2 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3420–3460m/s
Mechanical loss coefficient (tan delta)3.31e-4–8.16e-4 

CuZn30Pb2 Processing properties

Metal castingAcceptable
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed94.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn30Pb2 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)
Notes: Contains lead which lubricates, improving resistance.
Excellent
FlammabilityNon-flammable

CuZn30Pb2 C85400 Sand-Cast Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn30Pb2 Notes

CuZn30Pb2 C85400 Sand-Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn30Pb2 Standards with similar compositions

Australia: 854C to AS 1565, C85400 to AS 2738
USA: C85400, C85400 to ASTM B271, C85400 to ASTM B30, C85400 to ASTM B584, C85400 to ASTM B763, C85400 to QQ C-390, C85400 to SAE J462, UNS C85400