Home » Brass Alloys » CuZn40Pb2 (C38000) Brass, Pressure Die Cast Material Data Sheet
CuZn40Pb2 (C38000) Brass, Pressure Die Cast Material Data Sheet
CuZn40Pb2 (C38000) Brass Material Data Sheet (Cast, Pressure Die Cast)
CuZn40Pb2 C38000 Pressure Die Cast Overview
CuZn40Pb2 C38000 pressure die cast is a cast brass (UNS C38000). Condition: Pressure Die Cast. This CuZn40Pb2 C38000 pressure die cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn40Pb2 brass castings from Turkey (Türkiye)? Modulus Metal supplies CuZn40Pb2 brass castings with in-house CNC machining and inspects them before shipment.
CuZn40Pb2 Designation
CuZn40Pb2
UNS number
C38000
CuZn40Pb2 Typical uses
Accurate general-purpose pressure-cast items, free-cutting.
CuZn40Pb2 C38000 Pressure Die Cast Composition detail
Al (aluminum)
0
–
0.5
%
Cu (copper)
52.8
–
62.1
%
Fe (iron)
0
–
0.35
%
Pb (lead)
1.5
–
2.5
%
Sn (tin)
0
–
0.3
%
Zn (zinc)
36.4
–
43.5
%
CuZn40Pb2 Physical properties
Density
7.92
–
8.08
g/cm3
CuZn40Pb2 C38000 Pressure Die Cast Mechanical properties
Young’s modulus
91.1
–
92.9
GPa
Specific stiffness
11.3
–
11.7
MN.m/kg
Yield strength (elastic limit)
90
–
120
MPa
Tensile strength
280
–
370
MPa
Specific strength
11.2
–
15
kN.m/kg
Elongation
25
–
40
% strain
Compressive strength
90
–
120
MPa
Flexural modulus
91.1
–
92.9
GPa
Flexural strength (modulus of rupture)
90
–
120
MPa
Shear modulus
33.7
–
34.4
GPa
Bulk modulus
98.4
–
100
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
29
Hardness – Vickers
60
–
70
HV
Elastic stored energy (springs)
44.8
–
76.9
kJ/m3
Fatigue strength at 10^7 cycles
140
–
168
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
116
–
203
MPa
CuZn40Pb2 Impact & fracture properties
Fracture toughness
70.4
–
79.2
MPa.m0.5
Toughness (G)
54
–
68
kJ/m2
CuZn40Pb2 C38000 Pressure Die Cast Thermal properties
Melting point
882
–
902
°C
Maximum service temperature
120
–
130
°C
Minimum service temperature
-273
°C
Thermal conductivity
122
–
129
W/m.°C
Specific heat capacity
373
–
375
J/kg.°C
Thermal expansion coefficient
20.1
–
20.5
µstrain/°C
Thermal shock resistance
48.2
–
64.3
°C
Thermal distortion resistance
6
–
6.37
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn40Pb2 Electrical properties
Electrical resistivity
9.12
–
10
µohm.cm
Electrical conductivity
17.2
–
18.9
%IACS
Galvanic potential
-0.36
–
-0.28
V
CuZn40Pb2 Magnetic properties
Magnetic type
Non-magnetic
CuZn40Pb2 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3370
–
3420
m/s
Mechanical loss coefficient (tan delta)
2.78e-4
–
4.94e-4
CuZn40Pb2 Processing properties
Metal casting
Acceptable
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
94.5 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor
CuZn40Pb2 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn40Pb2 C38000 Pressure Die Cast Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn40Pb2 Notes
CuZn40Pb2 C38000 Pressure Die Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn40Pb2 Standards with similar compositions
Europe: CB755S to CEN EN 1982, CC755S to CEN EN 1982