Home » Brass Alloys » CuZn36 (C26800) Basis Brass, Hard Material Data Sheet
CuZn36 (C26800) Basis Brass, Hard Material Data Sheet
CuZn36 (C26800) Basis Brass Material Data Sheet (Wrought, Hard)
CuZn36 C26800 Hard Overview
CuZn36 C26800 hard is a wrought brass (UNS C26800), known as basis brass. Condition: Hard. This CuZn36 C26800 hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn36 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn36 brass parts in-house and inspects them before shipment.
CuZn36 Designation
CuZn36, wrought
Condition
Hard
UNS number
C26800
EN name
CW506L
ISO name
CuZn33
JIS (Japanese) name
C2680
CuZn36 Typical uses
Good general cold-working alloy for spinnings & presswork but not deep-drawn items, cold-headed components, springs, car radiator tanks, hardware, fasteners, electrical items, wire brushes etc.
CuZn36 C26800 Hard Composition detail
Cu (copper)
64
–
68.5
%
Fe (iron)
0
–
0.05
%
Pb (lead)
0
–
0.15
%
Zn (zinc)
31.3
–
36
%
CuZn36 Physical properties
Density
8.33
–
8.5
g/cm3
CuZn36 C26800 Hard Mechanical properties
Young’s modulus
97
–
103
GPa
Specific stiffness
11.5
–
12.3
MN.m/kg
Yield strength (elastic limit)
170
–
180
MPa
Tensile strength
515
–
530
MPa
Specific strength
20.2
–
21.4
kN.m/kg
Elongation
4
–
5
% strain
Compressive strength
170
–
180
MPa
Flexural modulus
97
–
103
GPa
Flexural strength (modulus of rupture)
170
–
180
MPa
Shear modulus
35.9
–
38.1
GPa
Bulk modulus
105
–
111
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
28
Hardness – Vickers
150
–
160
HV
Elastic stored energy (springs)
144
–
163
kJ/m3
Fatigue strength at 10^7 cycles
208
–
212
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
204
–
217
MPa
CuZn36 Impact & fracture properties
Fracture toughness
57.6
–
59.4
MPa.m0.5
Toughness (G)
32.8
–
35.7
kJ/m2
CuZn36 C26800 Hard Thermal properties
Melting point
902
–
919
°C
Maximum service temperature
200
–
210
°C
Minimum service temperature
-273
°C
Thermal conductivity
120
–
128
W/m.°C
Specific heat capacity
378
–
380
J/kg.°C
Thermal expansion coefficient
19
–
20.2
µstrain/°C
Thermal shock resistance
84.9
–
94
°C
Thermal distortion resistance
6.05
–
6.61
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn36 Electrical properties
Electrical resistivity
6.46
–
6.92
µohm.cm
Electrical conductivity
24.9
–
26.7
%IACS
Galvanic potential
-0.32
–
-0.24
V
CuZn36 Magnetic properties
Magnetic type
Non-magnetic
CuZn36 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3390
–
3500
m/s
Mechanical loss coefficient (tan delta)
1.23e-4
–
1.38e-4
CuZn36 Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Excellent
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
57.9 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor
CuZn36 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn36 C26800 Hard Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn36 Notes
CuZn36 C26800 Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn36 Standards with similar compositions
Australia: C26800 to AS 2738, C27000 to AS 2738
Canada: HC.4.Z34(268) to CSA HC.4.2
France: CuZn33 to NF A51-101, CuZn33 to NF A51-104
International: CuZn33 to ISO 1634, CuZn33 to ISO 1638, CuZn33 to ISO 426-1
Japan: C2680 P/R to JIS H3100, C2680 TW to JIS H3320, C2700 BD to JIS H3250, C2700 BE to JIS H3250, C2700 T to JIS H3300, C2700 W to JIS H3260
UK: CZ107 to BS 2870, CZ107 to BS 2873
USA: 65.5Cu-35.5Zn to AMS 4555, 65Cu-35Zn to QQ B-613, 65Cu-35Zn to QQ W-321, C26800, C26800 to ASTM B36/B36M, C26800 to ASTM B587, C26800 to SAE J463, C27000, C27000 to AMS 4712E, C27000 to ASTM B134, C27000 to ASTM B135M, C27000 to ASTM B587, C27000 to SAE J463, UNS C26800, UNS C27000