CuZn30 (C43600) Arsenical 70/30 Brass, Hard Material Data Sheet

CuZn30 (C43600) Arsenical 70/30 Brass Material Data Sheet (Wrought, Hard)

CuZn30 C43600 Hard Overview

CuZn30 C43600 hard is a wrought brass (UNS C43600), known as arsenical 70/30 brass. Condition: Hard. This CuZn30 C43600 hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn30 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn30 brass parts in-house and inspects them before shipment.

CuZn30 Designation

CuZn30, wrought
ConditionHard
EN nameCW701R
ISO nameCuZn19Sn
JIS (Japanese) nameC4350

CuZn30 Typical uses

Standard for condenser tubes, the arsenic inhibits dezincification.

CuZn30 C43600 Hard Composition detail

As (arsenic)0–0.06%
Cu (copper)69.9  %
Zn (zinc)30  %

CuZn30 Physical properties

Density8.38–8.55g/cm3

CuZn30 C43600 Hard Mechanical properties

Young’s modulus102–108GPa
Specific stiffness12–12.8MN.m/kg
Yield strength (elastic limit)380–460MPa
Tensile strength465–505MPa
Specific strength44.9–54.4kN.m/kg
Elongation10–20% strain
Compressive strength380–460MPa
Flexural modulus102–108GPa
Flexural strength (modulus of rupture)380–460MPa
Shear modulus37.7–40GPa
Bulk modulus110–117GPa
Poisson’s ratio0.34–0.35 
Shape factor19
Hardness – Vickers165–180HV
Elastic stored energy (springs)692–1000kJ/m3
Fatigue strength at 10^7 cycles195–206MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
181–222MPa

CuZn30 Impact & fracture properties

Fracture toughness31.1–35.8MPa.m0.5
Toughness (G)9.24–12.2kJ/m2

CuZn30 C43600 Hard Thermal properties

Melting point952–967°C
Maximum service temperature180–190°C
Minimum service temperature-200  °C
Thermal conductivity118–124W/m.°C
Specific heat capacity378–380J/kg.°C
Thermal expansion coefficient18.4–19.6µstrain/°C
Thermal shock resistance189–233°C
Thermal distortion resistance6.12–6.63MW/m
Latent heat of fusion220–240kJ/kg

CuZn30 Electrical properties

Electrical resistivity7.94–8.51µohm.cm
Electrical conductivity20.3–21.7%IACS
Temperature dependence of resistivity2.5–3.5/°C
Galvanic potential-0.3–-0.22V

CuZn30 Magnetic properties

Magnetic typeNon-magnetic

CuZn30 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3470–3580m/s
Mechanical loss coefficient (tan delta)1.9e-5–2.8e-5 

CuZn30 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingExcellent
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed57.9 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Poor

CuZn30 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn30 C43600 Hard Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn30 Notes

CuZn30 C43600 Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn30 Standards with similar compositions

Australia: 259 to AS 1567, 259 to AS 1572, C26130 to AS 2738
Europe: CW707R to CEN EN 12451
South Africa: Cu-Zn30As to SABS 460
UK: CZ105 to BS 2875, CZ126 to BS 2871
USA: C26130, C26130 to ASTM B569, UNS C26130
Tradenames: IMI 276, OLIN ARSENIC INHIBITED CARTRIDGE BRASS, SEVA (70/30 BRASS), TRIANGLE 171