Home » Brass Alloys » CuZn40Mn3Al2Fe2 (C86550) High-Tensile Manganese Bronze, Cast Material Data Sheet
CuZn40Mn3Al2Fe2 (C86550) High-Tensile Manganese Bronze, Cast Material Data Sheet
CuZn40Mn3Al2Fe2 (C86550) High-Tensile Manganese Bronze Material Data Sheet (Cast)
CuZn40Mn3Al2Fe2 C86550 Cast Overview
CuZn40Mn3Al2Fe2 C86550 cast is a cast brass (UNS C86550), known as high-tensile manganese bronze. Condition: Cast. This CuZn40Mn3Al2Fe2 C86550 cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn40Mn3Al2Fe2 brass castings from Turkey (Türkiye)? Modulus Metal supplies CuZn40Mn3Al2Fe2 brass castings with in-house CNC machining and inspects them before shipment.
CuZn40Mn3Al2Fe2 Designation
CuZn40Mn3Al2Fe2
UNS number
C86550
EN name
BS1400 HTB1
ISO name
CuZn40Mn3Al2Fe2
JIS (Japanese) name
CAC302 to JIS H5120, CAC302C to JIS H5121
CuZn40Mn3Al2Fe2 Typical uses
Highly-stressed components at normal temperature e.g.. marine propellers, rudders, pumps, hydraulic equipment, axleboxes, mountings, diecastings.
CuZn40Mn3Al2Fe2 C86550 Cast Composition detail
Al (aluminum)
0.5
–
2.5
%
Cu (copper)
57
–
60
%
Fe (iron)
0.7
–
2
%
Mn (manganese)
0.1
–
3
%
Ni (nickel)
0
–
1
%
Pb (lead)
0
–
0.5
%
Si (silicon)
0
–
0.1
%
Sn (tin)
0
–
1
%
Zn (zinc)
30
–
42
%
CuZn40Mn3Al2Fe2 Physical properties
Density
7.82
–
7.98
g/cm3
CuZn40Mn3Al2Fe2 C86550 Cast Mechanical properties
Young’s modulus
89.1
–
90.9
GPa
Specific stiffness
11.2
–
11.6
MN.m/kg
Yield strength (elastic limit)
210
–
280
MPa
Tensile strength
500
–
570
MPa
Specific strength
26.6
–
35.5
kN.m/kg
Elongation
18
–
35
% strain
Compressive strength
210
–
280
MPa
Flexural modulus
89.1
–
90.9
GPa
Flexural strength (modulus of rupture)
210
–
280
MPa
Shear modulus
33
–
33.6
GPa
Bulk modulus
96.2
–
98.2
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
24
Hardness – Vickers
100
–
150
HV
Elastic stored energy (springs)
249
–
428
kJ/m3
Fatigue strength at 10^7 cycles
204
–
223
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
182
–
250
MPa
CuZn40Mn3Al2Fe2 Impact & fracture properties
Fracture toughness
44.2
–
52.8
MPa.m0.5
Toughness (G)
21.9
–
30.8
kJ/m2
CuZn40Mn3Al2Fe2 C86550 Cast Thermal properties
Melting point
882
–
902
°C
Maximum service temperature
150
–
160
°C
Minimum service temperature
-273
°C
Thermal conductivity
83.1
–
90.1
W/m.°C
Specific heat capacity
372
–
374
J/kg.°C
Thermal expansion coefficient
20.3
–
20.7
µstrain/°C
Thermal shock resistance
114
–
152
°C
Thermal distortion resistance
4.05
–
4.4
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn40Mn3Al2Fe2 Electrical properties
Electrical resistivity
7.4
–
7.7
µohm.cm
Electrical conductivity
22.4
–
23.3
%IACS
Galvanic potential
-0.36
–
-0.28
V
CuZn40Mn3Al2Fe2 Magnetic properties
Magnetic type
Non-magnetic
CuZn40Mn3Al2Fe2 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3350
–
3400
m/s
Mechanical loss coefficient (tan delta)
5.1e-5
–
9.1e-5
CuZn40Mn3Al2Fe2 Processing properties
Metal casting
Excellent
Metal cold forming
Unsuitable
Metal hot forming
Unsuitable
Metal press forming
Unsuitable
Metal deep drawing
Unsuitable
Machining speed
79.2 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor
CuZn40Mn3Al2Fe2 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn40Mn3Al2Fe2 C86550 Cast Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn40Mn3Al2Fe2 Notes
CuZn40Mn3Al2Fe2 C86550 Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn40Mn3Al2Fe2 Standards with similar compositions
Germany: 2.0592 to DIN, 2.0602 to DIN 17656, GB-CuZn35Al1 to DIN 17656, G-CuZn35Al1 to DIN