Home » Brass Alloys » CuZn15As0.2 (C23000) Brazable Brass, Sand-Cast Material Data Sheet
CuZn15As0.2 (C23000) Brazable Brass Material Data Sheet (Cast, Sand-Cast)
CuZn15As0.2 C23000 Sand-Cast Overview
CuZn15As0.2 C23000 sand-cast is a cast brass (UNS C23000), known as brazable brass. Condition: Sand-Cast. This CuZn15As0.2 C23000 sand-cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn15As0.2 brass castings from Turkey (Türkiye)? Modulus Metal supplies CuZn15As0.2 brass castings with in-house CNC machining and inspects them before shipment.
CuZn15As0.2 Designation
CuZn15As0.2 UNS number C23000 EN name CW502L ISO name CuZn15 GB (Chinese) name H85 JIS (Japanese) name C2300
CuZn15As0.2 Typical uses
Marine fittings etc. to be brazed, flanges & end-plates, costume jewelry.
CuZn15As0.2 C23000 Sand-Cast Composition detail
Al (aluminum) 0 – 0.01 % As (arsenic) 0.05 – 0.2 % Cu (copper) 83 – 88 % Fe (iron) 0 – 0.15 % Mn (manganese) 0 – 0.1 % Ni (nickel) 0 – 0.1 % Pb (lead) 0 – 0.5 % Si (silicon) 0 – 0.02 % Sn (tin) 0 – 0.3 % Zn (zinc) 11.3 – 17 %
CuZn15As0.2 Physical properties
CuZn15As0.2 C23000 Sand-Cast Mechanical properties
Young’s modulus 99 – 101 GPa Specific stiffness 11.5 – 11.8 MN.m/kg Yield strength (elastic limit) 80 – 110 MPa Tensile strength 170 – 190 MPa Specific strength 9.3 – 12.8 kN.m/kg Elongation 18 – 40 % strain Compressive strength 80 – 110 MPa Flexural modulus 99 – 101 GPa Flexural strength (modulus of rupture) 80 – 110 MPa Shear modulus 36.6 – 37.4 GPa Bulk modulus 107 – 109 GPa Poisson’s ratio 0.34 – 0.35 Shape factor 30 Hardness – Vickers 45 – 60 HV Elastic stored energy (springs) 32.7 – 59.2 kJ/m3 Fatigue strength at 10^7 cycles 101 – 109 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 89.3 – 123 MPa
CuZn15As0.2 Impact & fracture properties
Fracture toughness 73.1 – 82.6 MPa.m0.5 Toughness (G) 53.6 – 68 kJ/m2
CuZn15As0.2 C23000 Sand-Cast Thermal properties
Melting point 1010 – 1020 °C Maximum service temperature 120 – 130 °C Minimum service temperature -273 °C Thermal conductivity 156 – 161 W/m.°C Specific heat capacity 380 – 382 J/kg.°C Thermal expansion coefficient 17.8 – 18.2 µstrain/°C Thermal shock resistance 44.4 – 61.1 °C Thermal distortion resistance 8.64 – 8.97 MW/m Latent heat of fusion 220 – 240 kJ/kg
CuZn15As0.2 Electrical properties
Electrical resistivity 5.89 – 6.92 µohm.cm Electrical conductivity 24.9 – 29.3 %IACS Galvanic potential -0.25 – -0.17 V
CuZn15As0.2 Magnetic properties
Magnetic type Non-magnetic
CuZn15As0.2 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3390 – 3430 m/s Mechanical loss coefficient (tan delta) 3.31e-4 – 6.25e-4
CuZn15As0.2 Processing properties
Metal casting Acceptable Metal cold forming Unsuitable Metal hot forming Unsuitable Metal press forming Unsuitable Metal deep drawing Unsuitable Machining speed 76.2 m/min Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements Good
CuZn15As0.2 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Acceptable Strong acids Unacceptable Weak alkalis Excellent Strong alkalis Excellent Organic solvents Excellent Oxidation at 500C Limited use UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Excellent Flammability Non-flammable
CuZn15As0.2 C23000 Sand-Cast Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide Susceptible
CuZn15As0.2 Notes
CuZn15As0.2 C23000 Sand-Cast Other notes (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn15As0.2 Standards with similar compositions
Australia: 837D to AS 1565, C83700 to AS 2738Europe: CB760S to CEN EN 1982, CC760S to CEN EN 1982Germany: 2.0241 to DIN, G-CuZn15 to DINSouth Africa: Cu-Zn14 to SABS 200USA: UNS C83700
Brass Alloys
CuZn15As0.2 (C23000) Material Data Sheets
Cast Sand-Cast You are here
All Brass Grades
Modulus Metal Services
Manufacturing & Quality Services in Turkey