CuZn35Sn1 (C85700) Naval Brass, Sand-Cast Material Data Sheet

CuZn35Sn1 (C85700) Naval Brass Material Data Sheet (Cast, Sand-Cast)

CuZn35Sn1 C85700 Sand-Cast Overview

CuZn35Sn1 C85700 sand-cast is a cast brass (UNS C85700), known as naval brass. Condition: Sand-Cast. This CuZn35Sn1 C85700 sand-cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn35Sn1 brass castings from Turkey (Türkiye)? Modulus Metal supplies CuZn35Sn1 brass castings with in-house CNC machining and inspects them before shipment.

CuZn35Sn1 Designation

CuZn35Sn1
UNS numberC85700
US nameC85700 to ASTM B584, ASTM B30, ASTM B763, ASTM B505, ASTM B271
ISO nameCuZn35Pb1Sn1

CuZn35Sn1 Typical uses

Marine fittings, pumps, fastenings, heat exchangers, machined items.

CuZn35Sn1 C85700 Sand-Cast Composition detail

Al (aluminum)0–0.8%
Cu (copper)58–64%
Fe (iron)0–0.7%
Ni (nickel)0–1%
Pb (lead)0.8–1.5%
Si (silicon)0–0.05%
Sn (tin)0.5–1.5%
Zn (zinc)32–40%

CuZn35Sn1 Physical properties

Density8.07–8.23g/cm3

CuZn35Sn1 C85700 Sand-Cast Mechanical properties

Young’s modulus95–97GPa
Specific stiffness11.6–11.9MN.m/kg
Yield strength (elastic limit)70–110MPa
Tensile strength250–310MPa
Specific strength8.59–13.5kN.m/kg
Elongation18–40% strain
Compressive strength70–110MPa
Flexural modulus95–97GPa
Flexural strength (modulus of rupture)70–110MPa
Shear modulus35.2–35.9GPa
Bulk modulus103–105GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers50–75HV
Elastic stored energy (springs)26.6–60.4kJ/m3
Fatigue strength at 10^7 cycles130–150MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
110–177MPa

CuZn35Sn1 Impact & fracture properties

Fracture toughness73.1–86.4MPa.m0.5
Toughness (G)56–77.3kJ/m2

CuZn35Sn1 C85700 Sand-Cast Thermal properties

Melting point917–932°C
Maximum service temperature120–130°C
Minimum service temperature-273  °C
Thermal conductivity80.5–87.3W/m.°C
Specific heat capacity375–377J/kg.°C
Thermal expansion coefficient18.8–19.2µstrain/°C
Thermal shock resistance38.4–60.3°C
Thermal distortion resistance4.23–4.6MW/m
Latent heat of fusion220–240kJ/kg

CuZn35Sn1 Electrical properties

Electrical resistivity7.6–8µohm.cm
Electrical conductivity21.6–22.7%IACS
Galvanic potential-0.34–-0.26V

CuZn35Sn1 Magnetic properties

Magnetic typeNon-magnetic

CuZn35Sn1 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3410–3460m/s
Mechanical loss coefficient (tan delta)3.31e-4–8.16e-4 

CuZn35Sn1 Processing properties

Metal castingAcceptable
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed85.3 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn35Sn1 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn35Sn1 C85700 Sand-Cast Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn35Sn1 Notes

CuZn35Sn1 C85700 Sand-Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn35Sn1 Standards with similar compositions

France: U-Z40-Y30 to NF A53-703
South Africa: Cu-Zn40 to SABS 200
Sweden: 5253-06 to SIS 145253
USA: C85700, C85700 to ASTM B176, C85700 to ASTM B271, C85700 to ASTM B30, C85700 to ASTM B505, C85700 to ASTM B584, C85700 to ASTM B763, UNS C85700