Home » Brass Alloys » CuZn40Pb1 (C36500) Leaded Muntz Metal, Cold Worked Material Data Sheet
CuZn40Pb1 (C36500) Leaded Muntz Metal, Cold Worked Material Data Sheet
CuZn40Pb1 (C36500) Leaded Muntz Metal Material Data Sheet (Wrought, Cold Worked)
CuZn40Pb1 C36500 Cold Worked Overview
CuZn40Pb1 C36500 cold worked is a wrought brass (UNS C36500), known as leaded muntz metal. Condition: Cold worked. This CuZn40Pb1 C36500 cold worked material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn40Pb1 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn40Pb1 brass parts in-house and inspects them before shipment.
CuZn40Pb1 Designation
CuZn40Pb1, wrought
Condition
Cold worked
UNS number
C36500
EN name
CW610N
ISO name
CuZn40Pb
GB (Chinese) name
HPb61-1
CuZn40Pb1 Typical uses
Condenser tube plates, porthole casings, extrusions, hot forgings, decorative brassware.
CuZn40Pb1 C36500 Cold Worked Composition detail
Cu (copper)
57.1
–
61.8
%
Fe (iron)
0
–
0.15
%
Pb (lead)
0.25
–
0.7
%
Sn (tin)
0
–
0.25
%
Zn (zinc)
37.9
–
41.8
%
CuZn40Pb1 Physical properties
Density
8.18
–
8.35
g/cm3
CuZn40Pb1 C36500 Cold Worked Mechanical properties
Young’s modulus
97
–
103
GPa
Specific stiffness
11.7
–
12.5
MN.m/kg
Yield strength (elastic limit)
240
–
400
MPa
Tensile strength
420
–
520
MPa
Specific strength
29
–
48.4
kN.m/kg
Elongation
5
–
30
% strain
Compressive strength
240
–
400
MPa
Flexural modulus
97
–
103
GPa
Flexural strength (modulus of rupture)
240
–
400
MPa
Shear modulus
35.9
–
38.1
GPa
Bulk modulus
105
–
111
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
23
Hardness – Vickers
110
–
145
HV
Elastic stored energy (springs)
303
–
760
kJ/m3
Fatigue strength at 10^7 cycles
183
–
210
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
153
–
252
MPa
CuZn40Pb1 Impact & fracture properties
Fracture toughness
34.5
–
48.7
MPa.m0.5
Toughness (G)
12.2
–
23.2
kJ/m2
CuZn40Pb1 C36500 Cold Worked Thermal properties
Melting point
882
–
902
°C
Maximum service temperature
97
–
110
°C
Minimum service temperature
-273
°C
Thermal conductivity
120
–
128
W/m.°C
Specific heat capacity
376
–
378
J/kg.°C
Thermal expansion coefficient
19.4
–
20.6
µstrain/°C
Thermal shock resistance
120
–
201
°C
Thermal distortion resistance
5.93
–
6.48
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn40Pb1 Electrical properties
Electrical resistivity
8.32
–
8.91
µohm.cm
Electrical conductivity
19.4
–
20.7
%IACS
Galvanic potential
-0.35
–
-0.27
V
CuZn40Pb1 Magnetic properties
Magnetic type
Non-magnetic
CuZn40Pb1 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3420
–
3530
m/s
Mechanical loss coefficient (tan delta)
2.5e-5
–
6.9e-5
CuZn40Pb1 Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
70.1 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor
CuZn40Pb1 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn40Pb1 C36500 Cold Worked Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn40Pb1 Notes
CuZn40Pb1 C36500 Cold Worked Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn40Pb1 Standards with similar compositions
Australia: 365 to AS 1567, 365 to AS 1568, C36500 to AS 2738
Canada: HC.4.ZP391(365) to CSA
Denmark: 5163 to DS 3003
Europe: CW610N to CEN EN 12164, CW610N to CEN EN 12165, CW610N to CEN EN 12166, CW610N to CEN EN 12167, CW610N to CEN EN 12420, CW610N to CEN EN 1652, CW610N to CEN EN 1653
Finland: CuZn40Pb to SFS 2925
International: CuZn40Pb to ISO 1634, CuZn40Pb to ISO 1637, CuZn40Pb to ISO 1638, CuZn40Pb to ISO 426-2
Norway: 16140 to NS 16140
Sweden: 5163-00 to SIS 145163, 5163-04 to SIS 145163
UK: CZ123 to BS 2870, CZ123 to BS 2872, CZ123 to BS 2875
USA: C36500, C36500 to ASTM B124M, C36500 to ASTM B171/B171M, C36500 to ASTM B283, UNS C36500, UNS C36600