Home » Brass Alloys » CuZn20 (C24000) Low Brass, Soft Material Data Sheet
CuZn20 (C24000) Low Brass, Soft Material Data Sheet
CuZn20 (C24000) Low Brass Material Data Sheet (Wrought, Soft)
CuZn20 C24000 Soft Overview
CuZn20 C24000 soft is a wrought brass (UNS C24000), known as low brass. Condition: Soft. This CuZn20 C24000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn20 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn20 brass parts in-house and inspects them before shipment.
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
143
–
163
MPa
CuZn20 Impact & fracture properties
Fracture toughness
65.5
–
70.4
MPa.m0.5
Toughness (G)
37.2
–
43.2
kJ/m2
CuZn20 C24000 Soft Thermal properties
Melting point
982
–
997
°C
Maximum service temperature
200
–
210
°C
Minimum service temperature
-273
°C
Thermal conductivity
135
–
140
W/m.°C
Specific heat capacity
380
–
382
J/kg.°C
Thermal expansion coefficient
17.5
–
18.5
µstrain/°C
Thermal shock resistance
57.5
–
68.2
°C
Thermal distortion resistance
7.39
–
7.9
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn20 Electrical properties
Electrical resistivity
5.25
–
5.62
µohm.cm
Electrical conductivity
30.7
–
32.8
%IACS
Galvanic potential
-0.27
–
-0.19
V
CuZn20 Magnetic properties
Magnetic type
Non-magnetic
CuZn20 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3600
–
3710
m/s
Mechanical loss coefficient (tan delta)
2.04e-4
–
2.78e-4
CuZn20 Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Limited use
Metal press forming
Acceptable
Metal deep drawing
Acceptable
Machining speed
48.8 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
CuZn20 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn20 C24000 Soft Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn20 Notes
CuZn20 C24000 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn20 Standards with similar compositions
Australia: C24000 to AS 2738
Canada: HC.4.Z20(240) to CSA HC.4.2
Czech Republic: CuZn20 to CSN 423203
Denmark: 5114 to DS 3003
Finland: CuZn20 to SFS 2917
France: CuZn20 to NF A51-101, CuZn20 to NF A51-104
Germany: 2.025 to DIN, CuZn20 to DIN
International: CuZn20 to ISO 1634, CuZn20 to ISO 1638, CuZn20 to ISO 426-1
Japan: C2400 P/R to JIS H3100, C2400 W to JIS H3260
Norway: 16110 to NS 16110
Sweden: 5114-02 to SIS 145114, 5114-04 to SIS 145114, 5114-05 to SIS 145114
UK: CZ103 to BS 2870, CZ103 to BS 2873, CZ103 to BS 2874
USA: 80Cu-20Zn to QQ B-613, 80Cu-20Zn to QQ B-626, 80Cu-20Zn to QQ B-650, 80Cu-20Zn to QQ W-321, C24000, C24000 to ASTM B134, C24000 to ASTM B36/B36M, C24000 to SAE J463, C24080, UNS C24000, UNS C24080