CuZn27Al4.5 High-Tensile Brass, As Drawn Material Data Sheet

CuZn27Al4.5 High-Tensile Brass Material Data Sheet (Wrought, As Drawn)

CuZn27Al4.5 As Drawn Brass Overview

CuZn27Al4.5 as drawn brass is a wrought brass (CZ116), known as high-tensile brass. Condition: As drawn. This CuZn27Al4.5 as drawn brass material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn27Al4.5 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn27Al4.5 brass parts in-house and inspects them before shipment.

CuZn27Al4.5 Designation

CuZn27Al4.5, wrought
ConditionAs drawn
EN nameCZ116
TradenamesHT27

CuZn27Al4.5 Typical uses

Architectural sections, fixings, forgings, pump parts, pressure tubes.

CuZn27Al4.5 As Drawn Brass Composition detail

Al (aluminum)4–5%
Cu (copper)64–68%
Fe (iron)0.25–1.2%
Mn (manganese)0.3–2%
Zn (zinc)23.3–31.4%
Other0–0.5%

CuZn27Al4.5 Physical properties

Density8.23–8.4g/cm3

CuZn27Al4.5 As Drawn Brass Mechanical properties

Young’s modulus101–107GPa
Specific stiffness12.1–12.9MN.m/kg
Yield strength (elastic limit)290–310MPa
Tensile strength540–570MPa
Specific strength34.8–37.3kN.m/kg
Elongation12–15% strain
Compressive strength290–310MPa
Flexural modulus101–107GPa
Flexural strength (modulus of rupture)290–310MPa
Shear modulus37.4–39.6GPa
Bulk modulus109–116GPa
Poisson’s ratio0.34–0.35 
Shape factor24
Hardness – Vickers165–170HV
Elastic stored energy (springs)403–464kJ/m3
Fatigue strength at 10^7 cycles215–223MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
206–232MPa

CuZn27Al4.5 Impact & fracture properties

Fracture toughness41.3–43.2MPa.m0.5
Toughness (G)16.3–18.1kJ/m2

CuZn27Al4.5 As Drawn Brass Thermal properties

Melting point952–967°C
Maximum service temperature180–190°C
Minimum service temperature-170–-160°C
Thermal conductivity110–117W/m.°C
Specific heat capacity377–379J/kg.°C
Thermal expansion coefficient18.9–20.1µstrain/°C
Thermal shock resistance140–156°C
Thermal distortion resistance5.57–6.08MW/m
Latent heat of fusion220–240kJ/kg

CuZn27Al4.5 Electrical properties

Electrical resistivity7.59–8.13µohm.cm
Electrical conductivity21.2–22.7%IACS
Temperature dependence of resistivity2.5–3.5/°C
Galvanic potential-0.34–-0.26V

CuZn27Al4.5 Magnetic properties

Magnetic typeNon-magnetic

CuZn27Al4.5 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3480–3590m/s
Mechanical loss coefficient (tan delta)4.2e-5–4.8e-5 

CuZn27Al4.5 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingAcceptable
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed54.9 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good

CuZn27Al4.5 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn27Al4.5 As Drawn Brass Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn27Al4.5 Notes

CuZn27Al4.5 As Drawn Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn27Al4.5 Standards with similar compositions

UK: CZ116 to BS 2872, CZ116 to BS 2874
Tradenames: CERRO HT27, DELTA HT17, DELTA HT27, MCKECHNIE 65