CuZn38Mn1.5 High-Tensile Brass, Hot Worked Material Data Sheet

CuZn38Mn1.5 High-Tensile Brass Material Data Sheet (Wrought, Hot Worked)

CuZn38Mn1.5 Hot Worked Brass Overview

CuZn38Mn1.5 hot worked brass is a wrought brass (CZ115), known as high-tensile brass. Condition: Hot worked. This CuZn38Mn1.5 hot worked brass material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn38Mn1.5 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn38Mn1.5 brass parts in-house and inspects them before shipment.

CuZn38Mn1.5 Designation

CuZn38Mn1.5, wrought
ConditionHot worked
EN nameCZ115
TradenamesHT1

CuZn38Mn1.5 Typical uses

Architectural sections, fixings, forgings, pump parts, pressure tubes.

CuZn38Mn1.5 Hot Worked Brass Composition detail

Cu (copper)58  %
Fe (iron)0.75  %
Mn (manganese)1.5  %
Pb (lead)1  %
Sn (tin)0.75  %
Zn (zinc)38  %

CuZn38Mn1.5 Physical properties

Density8.189–8.36g/cm3

CuZn38Mn1.5 Hot Worked Brass Mechanical properties

Young’s modulus97–103GPa
Specific stiffness11.7–12.5MN.m/kg
Yield strength (elastic limit)140–150MPa
Tensile strength370–390MPa
Specific strength16.9–18.2kN.m/kg
Elongation33–35% strain
Compressive strength140–150MPa
Flexural modulus97–103GPa
Flexural strength (modulus of rupture)140–150MPa
Shear modulus35.9–38.1GPa
Bulk modulus105–111GPa
Poisson’s ratio0.34–0.35 
Shape factor29
Hardness – Vickers85–95HV
Elastic stored energy (springs)97.6–113kJ/m3
Fatigue strength at 10^7 cycles168–174MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
162–181MPa

CuZn38Mn1.5 Impact & fracture properties

Fracture toughness63.3–65.5MPa.m0.5
Toughness (G)39.7–43.4kJ/m2

CuZn38Mn1.5 Hot Worked Brass Thermal properties

Melting point877–900°C
Maximum service temperature97–110°C
Minimum service temperature-200  °C
Thermal conductivity120–125W/m.°C
Specific heat capacity376–378J/kg.°C
Thermal expansion coefficient19.4–20.6µstrain/°C
Thermal shock resistance68.7–76.6°C
Thermal distortion resistance5.91–6.35MW/m
Latent heat of fusion220–240kJ/kg

CuZn38Mn1.5 Electrical properties

Electrical resistivity7.59–8.13µohm.cm
Electrical conductivity21.2–22.7%IACS
Temperature dependence of resistivity2.5–3.5/°C
Galvanic potential-0.36–-0.28V

CuZn38Mn1.5 Magnetic properties

Magnetic typeNon-magnetic

CuZn38Mn1.5 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3420–3530m/s
Mechanical loss coefficient (tan delta)1.78e-4–2.04e-4 

CuZn38Mn1.5 Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed88.4 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn38Mn1.5 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn38Mn1.5 Hot Worked Brass Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn38Mn1.5 Notes

CuZn38Mn1.5 Hot Worked Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn38Mn1.5 Standards with similar compositions

Europe: CW722R to CEN EN 12164, CW722R to CEN EN 12165, CW722R to CEN EN 12167, CW722R to CEN EN 12168, CW722R to CEN EN 12420
Tradenames: CERRO HT1, DELTA HIGH TENSILE BRASS HT1, DELTA HT1, DELTA HT1 HIGH SPEED MACHINING ROD, IMI 333, MCKECHNIE 540