Home » Brass Alloys » CuZn34Pb1 (C34000) Leaded Clock Brass, Soft Material Data Sheet
CuZn34Pb1 (C34000) Leaded Clock Brass, Soft Material Data Sheet
CuZn34Pb1 (C34000) Leaded Clock Brass Material Data Sheet (Wrought, Soft)
CuZn34Pb1 C34000 Soft Overview
CuZn34Pb1 C34000 soft is a wrought brass (UNS C34000), known as leaded clock brass. Condition: Soft. This CuZn34Pb1 C34000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn34Pb1 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn34Pb1 brass parts in-house and inspects them before shipment.
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
145
–
162
MPa
CuZn34Pb1 Impact & fracture properties
Fracture toughness
70.4
–
73.1
MPa.m0.5
Toughness (G)
47.2
–
51.9
kJ/m2
CuZn34Pb1 C34000 Soft Thermal properties
Melting point
927
–
942
°C
Maximum service temperature
180
–
190
°C
Minimum service temperature
-170
–
-160
°C
Thermal conductivity
118
–
124
W/m.°C
Specific heat capacity
377
–
379
J/kg.°C
Thermal expansion coefficient
18.9
–
20.1
µstrain/°C
Thermal shock resistance
53.4
–
60.2
°C
Thermal distortion resistance
5.97
–
6.45
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn34Pb1 Electrical properties
Electrical resistivity
6.46
–
6.92
µohm.cm
Electrical conductivity
24.9
–
26.7
%IACS
Galvanic potential
-0.33
–
-0.25
V
CuZn34Pb1 Magnetic properties
Magnetic type
Non-magnetic
CuZn34Pb1 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3480
–
3590
m/s
Mechanical loss coefficient (tan delta)
2.78e-4
–
3.31e-4
CuZn34Pb1 Processing properties
Metal casting
Unsuitable
Metal cold forming
Acceptable
Metal hot forming
Limited use
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
79.2 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor
CuZn34Pb1 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn34Pb1 C34000 Soft Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn34Pb1 Notes
CuZn34Pb1 C34000 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn34Pb1 Standards with similar compositions
Canada: HC.4.ZP341 to CSA HC.4.3
Denmark: 5140 to DS 3003
Europe: CW600N to CEN EN 12164, CW600N to CEN EN 12166, CW600N to CEN EN 12167, CW600N to CEN EN 12449, CW600N to CEN EN 1652
Finland: CuZn36Pb1 to SFS 2923
International: CuZn36Pb1 to ISO 1634, CuZn36Pb1 to ISO 1637, CuZn36Pb1 to ISO 1638, CuZn36Pb1 to ISO 426-2
Norway: 16150 to NS 16150
South Africa: Cu-Zn36Pb1 to SABS 460
UK: CZ118 to BS 2870
USA: 65Cu-34Zn-1Pb to QQ B-613, 65Cu-34Zn-1Pb to QQ B-626, C34000, C34000 to ASTM B121/B121M, C34000 to ASTM B453M, C34000 to CDA Datasheet, C35000 to SAE J463, UNS C34000, UNS C34700
Tradenames: BOHNALLOY R64, BOHNOLLOY R65, DELTA TR4 HIGH SPEED MACHINING ROD, IMI 410, MEDIUM LEADED BRASS 229, MEDIUM LEADED BRASS-340, MUELLER 3470, NITTANY NO. 30, NITTANY NO. 35, NORANDA 3400, REVERE ALLOY NO. 340, REVERE NO. 234, RM 421, SCOVILL MATRIX BRASS 340, SVENSKA SM-1263, TITAN NO. 35, WESTERN ALLOY NO. 62, WESTERN MEDIUM LEADED BRASS #62, WIELAND-Z11