CuZn15 (C23000) Red Brass Material Data Sheet (Wrought, Soft)
CuZn15 C23000 Soft Overview
| CuZn15 C23000 soft is a wrought brass (UNS C23000), known as red brass. Condition: Soft. This CuZn15 C23000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn15 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn15 brass parts in-house and inspects them before shipment. |
CuZn15 Designation
| CuZn15, wrought | |
| Condition | Soft |
| UNS number | C23000 |
| EN name | CW502L |
| ISO name | CuZn15 |
| GB (Chinese) name | H85 |
| JIS (Japanese) name | C2300 |
CuZn15 Typical uses
| Architectural & decorative items, jewelry, enameled & brazed parts. |
CuZn15 C23000 Soft Composition detail
| Cu (copper) | 84 | – | 86 | % |
| Fe (iron) | 0 | – | 0.05 | % |
| Pb (lead) | 0 | – | 0.05 | % |
| Zn (zinc) | 13.9 | – | 16 | % |
CuZn15 Physical properties
| Density | 8.58 | – | 8.75 | g/cm3 |
CuZn15 C23000 Soft Mechanical properties
| Young’s modulus | 114 | – | 122 | GPa |
| Specific stiffness | 13.1 | – | 14.1 | MN.m/kg |
| Yield strength (elastic limit) | 120 | – | 130 | MPa |
| Tensile strength | 295 | – | 310 | MPa |
| Specific strength | 13.8 | – | 15 | kN.m/kg |
| Elongation | 38 | – | 40 | % strain |
| Compressive strength | 120 | – | 130 | MPa |
| Flexural modulus | 114 | – | 122 | GPa |
| Flexural strength (modulus of rupture) | 120 | – | 130 | MPa |
| Shear modulus | 42.2 | – | 45.1 | GPa |
| Bulk modulus | 123 | – | 132 | GPa |
| Poisson’s ratio | 0.34 | – | 0.35 | |
| Shape factor | 30 | |||
| Hardness – Vickers | 63 | – | 68 | HV |
| Elastic stored energy (springs) | 60.8 | – | 72 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 145 | – | 150 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 140 | – | 155 | MPa |
CuZn15 Impact & fracture properties
| Fracture toughness | 67.9 | – | 70.4 | MPa.m0.5 |
| Toughness (G) | 38.6 | – | 42.6 | kJ/m2 |
CuZn15 C23000 Soft Thermal properties
| Melting point | 1010 | – | 1020 | °C |
| Maximum service temperature | 200 | – | 210 | °C |
| Minimum service temperature | -273 | °C | ||
| Thermal conductivity | 156 | – | 161 | W/m.°C |
| Specific heat capacity | 381 | – | 383 | J/kg.°C |
| Thermal expansion coefficient | 17 | – | 18 | µstrain/°C |
| Thermal shock resistance | 57.1 | – | 64.2 | °C |
| Thermal distortion resistance | 8.77 | – | 9.36 | MW/m |
| Latent heat of fusion | 220 | – | 240 | kJ/kg |
CuZn15 Electrical properties
| Electrical resistivity | 4.47 | – | 4.79 | µohm.cm |
| Electrical conductivity | 36 | – | 38.6 | %IACS |
| Galvanic potential | -0.25 | – | -0.17 | V |
CuZn15 Magnetic properties
| Magnetic type | Non-magnetic |
CuZn15 Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 3620 | – | 3760 | m/s |
| Mechanical loss coefficient (tan delta) | 2.37e-4 | – | 2.78e-4 | |
CuZn15 Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Acceptable |
| Metal hot forming | Limited use |
| Metal press forming | Acceptable |
| Metal deep drawing | Acceptable |
| Machining speed | 45.7 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
CuZn15 Durability
| Water (fresh) | Excellent |
| Water (salt) | Excellent |
| Weak acids | Acceptable |
| Strong acids | Acceptable |
| Weak alkalis | Excellent |
| Strong alkalis | Excellent |
| Organic solvents | Excellent |
| Oxidation at 500C | Limited use |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Excellent |
| Flammability | Non-flammable |
CuZn15 C23000 Soft Corrosion resistance
| Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide | Susceptible |
CuZn15 Notes
| CuZn15 C23000 Soft Other notes |
| (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng. |
CuZn15 Standards with similar compositions
| Australia: 230 to AS 1566, C23000 to AS 2738 |
| Canada: HC.4.Z15(230) to CSA HC.4.2 |
| Czech Republic: CuZn15 to CSN 423202 |
| Denmark: 5112 to DS 3003 |
| Finland: CuZn15 to SFS 2916 |
| France: CuZn15 to NF A51-101, CuZn15 to NF A51-104 |
| Germany: 2.024 to DIN, CuZn15 to DIN |
| International: CuZn15 to ISO 1634, CuZn15 to ISO 1635, CuZn15 to ISO 1637, CuZn15 to ISO 1638, CuZn15 to ISO 426-1 |
| Japan: C2300 P/R to JIS H3100, C2300 to JIS H3300, C2300 W to JIS H3260 |
| Norway: 16108 to NS 16108 |
| Sweden: 5112-02 to SIS 145112, 5112-04 to SIS 145112, 5112-05 to SIS 145112 |
| UK: CZ102 to BS 2870, CZ102 to BS 2873 |
| USA: 85Cu-15Zn to MIL T-20168, 85Cu-15Zn to QQ B-613, 85Cu-15Zn to QQ B-626, 85Cu-15Zn to QQ W-321, C23000, C23000 to ASTM B111M, C23000 to ASTM B134, C23000 to ASTM B135M, C23000 to ASTM B359M, C23000 to ASTM B36/B36M, C23000 to ASTM B395M, C23000 to ASTM B43, C23000 to ASTM B543M, C23000 to ASTM B569, C23000 to ASTM B587, C23000 to ASTM B888, C23000 to SAE J463, UNS C23000 |
| Tradenames: 2300, 85/15 RICH LOW BRASS, ANACONDA 230, ANACONDA 85, BOLTOMET 514, BRAZING METAL F, BRIDGEPORT NO. 85, FUCHS 2185, IMI 215, MESSING 85, MUELLER 2300, OLIN RED BRASS, OUTOKUMPU MS85, PLUMRITE 85, PLUMRITE STANDARD 85, PRINCES METAL NO. 2, PRYM 223, RED BRASS, RED BRASS 230, RED BRASS, 85%, REVERE RED BRASS, RIVERSIDE 62, RM 215, SCOVILL RED BRASS, 85%, ALLOY 230, SEYMOUR 2285, SEYMOUR 285, SM-1085, TOMBAC, OKER, VOLCO NO. 10, WESTERN ALLOY NO. 15, WESTERN RED BRASS #15, WIELAND-M15, WOLVERINE ALLOY 28 |