UNS S32760 vs AISI 329

UNS S32760 vs AISI 329

PropertyUNS S32760 (1.4501 / F55 · Zeron 100)AISI 329 (S32900 · 1st generation)
COMPOSITION (%)
Cr (chromium)24 – 2623 – 28
Ni (nickel)6 – 82 – 5
Mo (molybdenum)3 – 41 – 2
N (nitrogen)0.2 – 0.3—
Cu (copper)0.5 – 1—
Mn (manganese)0 – 10 – 1
W (tungsten)0.5 – 1—
PHYSICAL
Density (g/cm3)7.73 – 7.827.7 – 7.9
MECHANICAL
Young’s Modulus (GPa)190 – 200189 – 204
Yield Strength (MPa)515 – 565500 – 600
Tensile Strength (MPa)700 – 930650 – 795
Elongation (% strain)23 – 2720 – 35
Hardness – Brinell (HB)276 – 286130 – 150
Hardness – Rockwell C280 – 4
Fatigue Strength @ 10^7 (MPa)241 – 267316 – 365
Fracture Toughness (MPa*m^0.5)150 – 19571 – 110
THERMAL
Melting Point (C)1400 – 14501380 – 1450
Max Service Temp (C)335 – 365740 – 787
Min Service Temp (C)-60 – -50-150
Thermal Conductivity (W/m*C)12.9 – 1515 – 21
CORROSION RESISTANCE
PREN37.9 – 45.726.3 – 34.6
Pitting & Crevice CorrosionVery High (>40)High (30-40)
Stress Corrosion CrackingSlightly SusceptibleSusceptible
Sea WaterExcellentModerate
Sour Oil & GasGoodModerate
PROCESSING
Machining Speed (m/min)14.625.6
WeldabilityGood (MIG/plasma/SAW/TIG: Excellent)Good (MIG/plasma/SAW/TIG: Good)
Metal CastingUnsuitableUnsuitable
Metal Hot FormingLimited useAcceptable
Carbon Equivalency1.12 – 1.40.867 – 1.29
NOTES
Generation / Notes2nd generation duplex1st generation duplex, no longer produced much
Typical Uses—Processing of potentially corrosive liquids (chemicals/oil/beverages/sewage); structural uses in corrosive environments e.g. nuclear plants, ships, offshore oil installations, underwater cables and pipes
Cast Grades
Wrought Grades