Home » Brass Alloys » CuZn28Sn1 (C44300) Admiralty Brass, Half Hard Material Data Sheet
CuZn28Sn1 (C44300) Admiralty Brass, Half Hard Material Data Sheet
CuZn28Sn1 (C44300) Admiralty Brass Material Data Sheet (Wrought, Half Hard)
CuZn28Sn1 C44300 Half Hard Overview
CuZn28Sn1 C44300 half hard is a wrought brass (UNS C44300), known as admiralty brass. Condition: Half hard. This CuZn28Sn1 C44300 half hard material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn28Sn1 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn28Sn1 brass parts in-house and inspects them before shipment.
CuZn28Sn1 Designation
CuZn28Sn1, wrought
Condition
Half hard
UNS number
C44300
EN name
CW706R
ISO name
CuZn28Sn1
GB (Chinese) name
HSn70-1
JIS (Japanese) name
C4430
CuZn28Sn1 Typical uses
Heat exchangers, especially for power stations & refineries.
CuZn28Sn1 C44300 Half Hard Composition detail
As (arsenic)
0.02
–
0.06
%
Cu (copper)
69.5
–
73.5
%
Fe (iron)
0
–
0.06
%
Pb (lead)
0
–
0.07
%
Sn (tin)
0.9
–
1.2
%
Zn (zinc)
25.6
–
29.1
%
CuZn28Sn1 Physical properties
Density
8.38
–
8.55
g/cm3
CuZn28Sn1 C44300 Half Hard Mechanical properties
Young’s modulus
102
–
108
GPa
Specific stiffness
12
–
12.8
MN.m/kg
Yield strength (elastic limit)
390
–
420
MPa
Tensile strength
400
–
520
MPa
Specific strength
46
–
49.7
kN.m/kg
Elongation
10
–
20
% strain
Compressive strength
390
–
420
MPa
Flexural modulus
102
–
108
GPa
Flexural strength (modulus of rupture)
390
–
420
MPa
Shear modulus
37.7
–
40
GPa
Bulk modulus
110
–
117
GPa
Poisson’s ratio
0.34
–
0.35
Shape factor
20
Hardness – Vickers
160
–
190
HV
Elastic stored energy (springs)
722
–
843
kJ/m3
Fatigue strength at 10^7 cycles
177
–
210
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
148
–
251
MPa
CuZn28Sn1 Impact & fracture properties
Fracture toughness
33.3
–
35.2
MPa.m0.5
Toughness (G)
10.5
–
11.9
kJ/m2
CuZn28Sn1 C44300 Half Hard Thermal properties
Melting point
952
–
967
°C
Maximum service temperature
180
–
190
°C
Minimum service temperature
-200
°C
Thermal conductivity
118
–
123
W/m.°C
Specific heat capacity
378
–
380
J/kg.°C
Thermal expansion coefficient
18.4
–
19.6
µstrain/°C
Thermal shock resistance
192
–
215
°C
Thermal distortion resistance
6.11
–
6.59
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn28Sn1 Electrical properties
Electrical resistivity
6.61
–
7.24
µohm.cm
Electrical conductivity
23.8
–
26.1
%IACS
Galvanic potential
-0.3
–
-0.22
V
CuZn28Sn1 Magnetic properties
Magnetic type
Non-magnetic
CuZn28Sn1 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3470
–
3580
m/s
Mechanical loss coefficient (tan delta)
2.3e-5
–
2.6e-5
CuZn28Sn1 Processing properties
Metal casting
Unsuitable
Metal cold forming
Limited use
Metal hot forming
Limited use
Metal press forming
Limited use
Metal deep drawing
Limited use
Machining speed
64 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
CuZn28Sn1 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn28Sn1 C44300 Half Hard Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn28Sn1 Notes
CuZn28Sn1 C44300 Half Hard Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn28Sn1 Standards with similar compositions
Australia: C44300 to AS 2738
Canada: HC.4.ZT281V(443) to CSA
Europe: CW706R to CEN EN 12451, CW706R to CEN EN 12452
Germany: 2.047 to DIN, CuZn28Sn1 to DIN
International: CuZn28Sn1 to ISO 1634, CuZn28Sn1 to ISO 1635, CuZn28Sn1 to ISO 426-1
Japan: C4430 P/R to JIS H3100, C4430 T to JIS H3300, C4430 TW to JIS H3320
South Africa: Cu-Zn28Sn1 to SABS 460
UK: CZ111 to BS 2871
USA: C44300, C44300 to ASTM B111M, C44300 to ASTM B135M, C44300 to ASTM B171/B171M, C44300 to ASTM B359M, C44300 to ASTM B395M, C44300 to ASTM B543M, C44300 to CDA Datasheet, UNS C44300