CuZn28Sn1 (C44300) Admiralty Brass, Soft Material Data Sheet

CuZn28Sn1 (C44300) Admiralty Brass Material Data Sheet (Wrought, Soft)

CuZn28Sn1 C44300 Soft Overview

CuZn28Sn1 C44300 soft is a wrought brass (UNS C44300), known as admiralty brass. Condition: Soft. This CuZn28Sn1 C44300 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn28Sn1 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn28Sn1 brass parts in-house and inspects them before shipment.

CuZn28Sn1 Designation

CuZn28Sn1, wrought
ConditionSoft
UNS numberC44300
EN nameCW706R
ISO nameCuZn28Sn1
GB (Chinese) nameHSn70-1
JIS (Japanese) nameC4430

CuZn28Sn1 Typical uses

Heat exchangers, especially for power stations & refineries.

CuZn28Sn1 C44300 Soft Composition detail

As (arsenic)0.02–0.06%
Cu (copper)69.5–73.5%
Fe (iron)0–0.06%
Pb (lead)0–0.07%
Sn (tin)0.9–1.2%
Zn (zinc)25.6–29.1%

CuZn28Sn1 Physical properties

Density8.38–8.55g/cm3

CuZn28Sn1 C44300 Soft Mechanical properties

Young’s modulus102–108GPa
Specific stiffness12–12.8MN.m/kg
Yield strength (elastic limit)100–110MPa
Tensile strength305–320MPa
Specific strength11.8–13kN.m/kg
Elongation58–60% strain
Compressive strength100–110MPa
Flexural modulus102–108GPa
Flexural strength (modulus of rupture)100–110MPa
Shear modulus37.7–40GPa
Bulk modulus110–117GPa
Poisson’s ratio0.34–0.35 
Shape factor30
Hardness – Vickers75–78HV
Elastic stored energy (springs)47.6–57.7kJ/m3
Fatigue strength at 10^7 cycles148–153MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
143–158MPa

CuZn28Sn1 Impact & fracture properties

Fracture toughness73.1–76MPa.m0.5
Toughness (G)50.5–55.5kJ/m2

CuZn28Sn1 C44300 Soft Thermal properties

Melting point952–967°C
Maximum service temperature180–190°C
Minimum service temperature-200  °C
Thermal conductivity118–123W/m.°C
Specific heat capacity378–380J/kg.°C
Thermal expansion coefficient18.4–19.6µstrain/°C
Thermal shock resistance49.4–56.1°C
Thermal distortion resistance6.11–6.59MW/m
Latent heat of fusion220–240kJ/kg

CuZn28Sn1 Electrical properties

Electrical resistivity6.61–7.24µohm.cm
Electrical conductivity23.8–26.1%IACS
Galvanic potential-0.3–-0.22V

CuZn28Sn1 Magnetic properties

Magnetic typeNon-magnetic

CuZn28Sn1 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3470–3580m/s
Mechanical loss coefficient (tan delta)3.31e-4–4e-4 

CuZn28Sn1 Processing properties

Metal castingUnsuitable
Metal cold formingLimited use
Metal hot formingLimited use
Metal press formingLimited use
Metal deep drawingAcceptable
Machining speed64 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good

CuZn28Sn1 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn28Sn1 C44300 Soft Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn28Sn1 Notes

CuZn28Sn1 C44300 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn28Sn1 Standards with similar compositions

Australia: C44300 to AS 2738
Canada: HC.4.ZT281V(443) to CSA
Europe: CW706R to CEN EN 12451, CW706R to CEN EN 12452
Germany: 2.047 to DIN, CuZn28Sn1 to DIN
International: CuZn28Sn1 to ISO 1634, CuZn28Sn1 to ISO 1635, CuZn28Sn1 to ISO 426-1
Japan: C4430 P/R to JIS H3100, C4430 T to JIS H3300, C4430 TW to JIS H3320
South Africa: Cu-Zn28Sn1 to SABS 460
UK: CZ111 to BS 2871
USA: C44300, C44300 to ASTM B111M, C44300 to ASTM B135M, C44300 to ASTM B171/B171M, C44300 to ASTM B359M, C44300 to ASTM B395M, C44300 to ASTM B543M, C44300 to CDA Datasheet, UNS C44300
Tradenames: 4430, ADMIRALTY BRASS, ADMIRALTY METAL, ANACONDA 443, ARSENICAL ADMIRALTY 30, ARSENICAL ADMIRALTY-443, BOOTH ADA, BRIDGEPORT NO. 30, MUELLER 4430, REVERE NO. 443, WIELAND-S28