Home » Brass Alloys » CuZn40 (C85500) Brass, Gravity Die-Cast Material Data Sheet
CuZn40 (C85500) Brass Material Data Sheet (Cast, Gravity Die-Cast)
CuZn40 C85500 Gravity Die-Cast Overview
CuZn40 C85500 gravity die-cast is a cast brass (UNS C85500). Condition: Gravity Die-Cast. This CuZn40 C85500 gravity die-cast material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn40 brass castings from Turkey (Türkiye)? Modulus Metal supplies CuZn40 brass castings with in-house CNC machining and inspects them before shipment.
CuZn40 Designation
CuZn40 UNS number C85500 EN name CW509L ISO name CuZn40 JIS (Japanese) name C2800 / C2801
CuZn40 Typical uses
Accurate, general-purpose castings, automobiles, plumbing & gas fittings.
CuZn40 C85500 Gravity Die-Cast Composition detail
Cu (copper) 58 – 64 % Fe (iron) 0 – 0.2 % Mn (manganese) 0 – 0.2 % Ni (nickel) 0 – 0.2 % Pb (lead) 0 – 0.2 % Sn (tin) 0 – 0.2 % Zn (zinc) 36 – 41 %
CuZn40 Physical properties
CuZn40 C85500 Gravity Die-Cast Mechanical properties
Young’s modulus 93.1 – 94.9 GPa Specific stiffness 11.4 – 11.8 MN.m/kg Yield strength (elastic limit) 90 – 120 MPa Tensile strength 280 – 370 MPa Specific strength 11.1 – 14.8 kN.m/kg Elongation 23 – 50 % strain Compressive strength 90 – 120 MPa Flexural modulus 93.1 – 94.9 GPa Flexural strength (modulus of rupture) 90 – 120 MPa Shear modulus 34.4 – 35.1 GPa Bulk modulus 101 – 103 GPa Poisson’s ratio 0.34 – 0.35 Shape factor 30 Hardness – Vickers 60 – 70 HV Elastic stored energy (springs) 43.9 – 75.2 kJ/m3 Fatigue strength at 10^7 cycles 140 – 168 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 114 – 207 MPa
CuZn40 Impact & fracture properties
Fracture toughness 70.4 – 79.2 MPa.m0.5 Toughness (G) 52.9 – 66.5 kJ/m2
CuZn40 C85500 Gravity Die-Cast Thermal properties
Melting point 882 – 902 °C Maximum service temperature 120 – 130 °C Minimum service temperature -273 °C Thermal conductivity 111 – 121 W/m.°C Specific heat capacity 374 – 376 J/kg.°C Thermal expansion coefficient 19.8 – 20.2 µstrain/°C Thermal shock resistance 47.9 – 63.9 °C Thermal distortion resistance 5.56 – 6.04 MW/m Latent heat of fusion 220 – 240 kJ/kg
CuZn40 Electrical properties
Electrical resistivity 6.5 – 6.8 µohm.cm Electrical conductivity 25.4 – 26.5 %IACS Galvanic potential -0.34 – -0.26 V
CuZn40 Magnetic properties
Magnetic type Non-magnetic
CuZn40 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3380 – 3430 m/s Mechanical loss coefficient (tan delta) 2.78e-4 – 4.94e-4
CuZn40 Processing properties
Metal casting Acceptable Metal cold forming Unsuitable Metal hot forming Unsuitable Metal press forming Unsuitable Metal deep drawing Unsuitable Machining speed 61 m/min Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements Poor
CuZn40 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Acceptable Strong acids Unacceptable Weak alkalis Excellent Strong alkalis Excellent Organic solvents Excellent Oxidation at 500C Limited use UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Excellent Flammability Non-flammable
CuZn40 C85500 Gravity Die-Cast Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide Highly susceptible
CuZn40 Notes
CuZn40 C85500 Gravity Die-Cast Other notes (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn40 Standards with similar compositions
USA: C85500, UNS C85500, UNS C85600Tradenames: DOLER-BRASS 2, LO-TEMP, MICHIGAN GRADE XXX, PRESSCO NO. 4, TOBIN BRONZE 470, WESTERN MUNTZ METAL