CuZn30Al5Mn4Fe2 High-Tensile Manganese Bronze, Cast Material Data Sheet

CuZn30Al5Mn4Fe2 High-Tensile Manganese Bronze Material Data Sheet (Cast)

CuZn30Al5Mn4Fe2 Cast Brass Overview

CuZn30Al5Mn4Fe2 cast brass is a cast brass, known as high-tensile manganese bronze. Condition: Cast. This CuZn30Al5Mn4Fe2 cast brass material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn30Al5Mn4Fe2 brass castings from Turkey (Türkiye)? Modulus Metal supplies CuZn30Al5Mn4Fe2 brass castings with in-house CNC machining and inspects them before shipment.

CuZn30Al5Mn4Fe2 Designation

CuZn30Al5Mn4Fe2

CuZn30Al5Mn4Fe2 Typical uses

Highly-stressed components not subject to stress corrosion e.g.. rolling mill castings, slow spur & gear wheels.

CuZn30Al5Mn4Fe2 Cast Brass Composition detail

Al (aluminum)3–6%
Cu (copper)57.8–61.5%
Fe (iron)1.5–2.25%
Mn (manganese)4  %
Zn (zinc)30  %

CuZn30Al5Mn4Fe2 Physical properties

Density7.82–7.98g/cm3

CuZn30Al5Mn4Fe2 Cast Brass Mechanical properties

Young’s modulus89.1–90.9GPa
Specific stiffness11.2–11.6MN.m/kg
Yield strength (elastic limit)400–500MPa
Tensile strength740–930MPa
Specific strength50.6–63.3kN.m/kg
Elongation13–21% strain
Compressive strength400–500MPa
Flexural modulus89.1–90.9GPa
Flexural strength (modulus of rupture)400–500MPa
Shear modulus33–33.6GPa
Bulk modulus96.2–98.2GPa
Poisson’s ratio0.34–0.35 
Shape factor17
Hardness – Vickers150–350HV
Elastic stored energy (springs)899–1370kJ/m3
Fatigue strength at 10^7 cycles264–306MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
226–358MPa

CuZn30Al5Mn4Fe2 Impact & fracture properties

Fracture toughness29.2–34.5MPa.m0.5
Toughness (G)9.53–13.1kJ/m2

CuZn30Al5Mn4Fe2 Cast Brass Thermal properties

Melting point952–967°C
Maximum service temperature150–160°C
Minimum service temperature-273  °C
Thermal conductivity34.1–36.9W/m.°C
Specific heat capacity372–374J/kg.°C
Thermal expansion coefficient21.2–22µstrain/°C
Thermal shock resistance205–258°C
Thermal distortion resistance1.57–1.72MW/m
Latent heat of fusion220–240kJ/kg

CuZn30Al5Mn4Fe2 Electrical properties

Electrical resistivity21.6–22.4µohm.cm
Electrical conductivity7.7–7.98%IACS
Galvanic potential-0.38–-0.3V

CuZn30Al5Mn4Fe2 Magnetic properties

Magnetic typeNon-magnetic

CuZn30Al5Mn4Fe2 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3350–3400m/s
Mechanical loss coefficient (tan delta)1.6e-5–2.5e-5 

CuZn30Al5Mn4Fe2 Processing properties

Metal castingExcellent
Metal cold formingUnsuitable
Metal hot formingUnsuitable
Metal press formingUnsuitable
Metal deep drawingUnsuitable
Machining speed64 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Poor

CuZn30Al5Mn4Fe2 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn30Al5Mn4Fe2 Cast Brass Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn30Al5Mn4Fe2 Notes

CuZn30Al5Mn4Fe2 Cast Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn30Al5Mn4Fe2 Standards with similar compositions

Tradenames: HOLFOS HTB 3, KRAMER XX MANGANESE BRONZE, LUMEN 19, MAGNALLOY 4231