Home » Brass Alloys » CuZn10Pb3Sn2 Brass, Sand-Cast Material Data Sheet
CuZn10Pb3Sn2 Brass Material Data Sheet (Cast, Sand-Cast)
CuZn10Pb3Sn2 Sand-Cast Brass Overview
CuZn10Pb3Sn2 sand-cast brass is a cast brass. Condition: Sand-Cast. This CuZn10Pb3Sn2 sand-cast brass material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn10Pb3Sn2 brass castings from Turkey (Türkiye)? Modulus Metal supplies CuZn10Pb3Sn2 brass castings with in-house CNC machining and inspects them before shipment.
CuZn10Pb3Sn2 Designation
CuZn10Pb3Sn2 Typical uses
Pressure-tight valves, cocks & fittings, hardware & ornamental, centrifugal castings.
CuZn10Pb3Sn2 Sand-Cast Brass Composition detail
Cu (copper) 84 – 87 % Pb (lead) 2 – 3 % Sn (tin) 1 – 3 % Zn (zinc) 10 %
CuZn10Pb3Sn2 Physical properties
CuZn10Pb3Sn2 Sand-Cast Brass Mechanical properties
Young’s modulus 97 – 99 GPa Specific stiffness 11.5 – 11.8 MN.m/kg Yield strength (elastic limit) 80 – 110 MPa Tensile strength 170 – 200 MPa Specific strength 9.52 – 13.1 kN.m/kg Elongation 18 – 40 % strain Compressive strength 80 – 110 MPa Flexural modulus 97 – 99 GPa Flexural strength (modulus of rupture) 80 – 110 MPa Shear modulus 35.9 – 36.6 GPa Bulk modulus 105 – 107 GPa Poisson’s ratio 0.34 – 0.35 Shape factor 30 Hardness – Vickers 45 – 60 HV Elastic stored energy (springs) 33.4 – 60.4 kJ/m3 Fatigue strength at 10^7 cycles 101 – 113 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 87.7 – 130 MPa
CuZn10Pb3Sn2 Impact & fracture properties
Fracture toughness 73.1 – 82.6 MPa.m0.5 Toughness (G) 54.7 – 69.4 kJ/m2
CuZn10Pb3Sn2 Sand-Cast Brass Thermal properties
Melting point 1030 – 1040 °C Maximum service temperature 120 – 130 °C Minimum service temperature -273 °C Thermal conductivity 185 – 192 W/m.°C Specific heat capacity 378 – 380 J/kg.°C Thermal expansion coefficient 18.3 – 18.7 µstrain/°C Thermal shock resistance 44.1 – 60.7 °C Thermal distortion resistance 9.98 – 10.4 MW/m Latent heat of fusion 220 – 240 kJ/kg
CuZn10Pb3Sn2 Electrical properties
Electrical resistivity 9.12 – 10 µohm.cm Electrical conductivity 17.2 – 18.9 %IACS Galvanic potential -0.25 – -0.17 V
CuZn10Pb3Sn2 Magnetic properties
Magnetic type Non-magnetic
CuZn10Pb3Sn2 Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 3390 – 3440 m/s Mechanical loss coefficient (tan delta) 3.31e-4 – 6.25e-4
CuZn10Pb3Sn2 Processing properties
Metal casting Acceptable Metal cold forming Unsuitable Metal hot forming Unsuitable Metal press forming Unsuitable Metal deep drawing Unsuitable Machining speed 70.1 m/min Weldability Unsuitable
CuZn10Pb3Sn2 Durability
Water (fresh) Excellent Water (salt) Excellent Weak acids Acceptable Strong acids Unacceptable Weak alkalis Excellent Strong alkalis Excellent Organic solvents Excellent Oxidation at 500C Limited use UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Notes: Contains lead which lubricates, improving resistance. Excellent Flammability Non-flammable
CuZn10Pb3Sn2 Sand-Cast Brass Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide Susceptible
CuZn10Pb3Sn2 Notes
CuZn10Pb3Sn2 Sand-Cast Other notes (s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn10Pb3Sn2 Standards with similar compositions
Tradenames: KRAMER 83-3-3-11 ALLOY, KRAMER 87-1-3-9 ALLOY, O.B. ALLOY NO. 5
Brass Alloys
CuZn10Pb3Sn2 Cast Material Data Sheets
Cast Sand-Cast You are here
All Brass Grades
Modulus Metal Services
Manufacturing & Quality Services in Turkey