CuZn40Pb3 (C37710) Free-Cutting Brass, Hot Worked Material Data Sheet

CuZn40Pb3 (C37710) Free-Cutting Brass Material Data Sheet (Wrought, Hot Worked)

CuZn40Pb3 C37710 Hot Worked Overview

CuZn40Pb3 C37710 hot worked is a wrought brass (UNS C37710), known as free-cutting brass. Condition: Hot worked. This CuZn40Pb3 C37710 hot worked material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn40Pb3 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn40Pb3 brass parts in-house and inspects them before shipment.

CuZn40Pb3 Designation

CuZn40Pb3, wrought
ConditionHot worked
UNS numberC37710
EN nameCW617N
ISO nameCuZn40Pb2

CuZn40Pb3 Typical uses

Machined parts on automatic lathes,, fasteners, bushes etc, extrusions, trim, fittings, terminals.

CuZn40Pb3 C37710 Hot Worked Composition detail

Cu (copper)54.2–62.3%
Fe (iron)0–0.3%
Pb (lead)1–3%
Zn (zinc)36.7–42.5%

CuZn40Pb3 Physical properties

Density8.18–8.35g/cm3

CuZn40Pb3 C37710 Hot Worked Mechanical properties

Young’s modulus97–103GPa
Specific stiffness11.7–12.5MN.m/kg
Yield strength (elastic limit)200–240MPa
Tensile strength430–460MPa
Specific strength24.2–29kN.m/kg
Elongation20–30% strain
Compressive strength200–240MPa
Flexural modulus97–103GPa
Flexural strength (modulus of rupture)200–240MPa
Shear modulus35.9–38.1GPa
Bulk modulus105–111GPa
Poisson’s ratio0.34–0.35 
Shape factor26
Hardness – Vickers100–150HV
Elastic stored energy (springs)201–287kJ/m3
Fatigue strength at 10^7 cycles185–194MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
173–207MPa

CuZn40Pb3 Impact & fracture properties

Fracture toughness48.7–54.3MPa.m0.5
Toughness (G)23.7–29.5kJ/m2

CuZn40Pb3 C37710 Hot Worked Thermal properties

Melting point877–897°C
Maximum service temperature180–190°C
Minimum service temperature-170–-160°C
Thermal conductivity118–124W/m.°C
Specific heat capacity376–378J/kg.°C
Thermal expansion coefficient19.4–20.6µstrain/°C
Thermal shock resistance99.2–121°C
Thermal distortion resistance5.82–6.29MW/m
Latent heat of fusion220–240kJ/kg

CuZn40Pb3 Electrical properties

Electrical resistivity5.89–6.46µohm.cm
Electrical conductivity26.7–29.3%IACS
Galvanic potential-0.35–-0.27V

CuZn40Pb3 Magnetic properties

Magnetic typeNon-magnetic

CuZn40Pb3 Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity3420–3530m/s
Mechanical loss coefficient (tan delta)6.9e-5–1e-4 

CuZn40Pb3 Processing properties

Metal castingUnsuitable
Metal cold formingAcceptable
Metal hot formingExcellent
Metal press formingAcceptable
Metal deep drawingLimited use
Machining speed94.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor

CuZn40Pb3 Durability

Water (fresh)Excellent
Water (salt)Excellent
Weak acidsAcceptable
Strong acidsUnacceptable
Weak alkalisExcellent
Strong alkalisExcellent
Organic solventsExcellent
Oxidation at 500CLimited use
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Excellent
FlammabilityNon-flammable

CuZn40Pb3 C37710 Hot Worked Corrosion resistance

Stress corrosion cracking
Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible

CuZn40Pb3 Notes

CuZn40Pb3 C37710 Hot Worked Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.

CuZn40Pb3 Standards with similar compositions

Australia: 377 to AS 1567, 377 to AS 1568, C37710 to AS 2738
Czech Republic: CuZn40Pb2 to CSN 423223
Denmark: 5168 to DS 3003
Finland: CuZn39Pb2 to SFS 2921
International: CuZn39Pb2 to ISO 1634, CuZn39Pb2 to ISO 1637, CuZn39Pb2 to ISO 1640, CuZn39Pb2 to ISO 426-2
Sweden: 5168-00 to SIS 145168, 5168-04 to SIS 145168, 5168-06 to SIS 145168
UK: CZ122 to BS 2872, CZ122 to BS 2874
USA: C37710, UNS C37710, UNS C37800
Tradenames: BOLTOMET 611, BOOTH B1, BOSCH (ME-1), BOSCH (ME-2), BRIDGEPORT NO. 133, CERRO S8, DELTA S1 FORGING ROD, DELTA S1 GENERAL PURPOSE ROD AND BAR, DELTA S1 HIGH SPEED MACHINING ROD, DELTA S8 FORGING ROD, DELTA S8 HIGH SPEED MACHINING ROD, F QUALITY, FUCHS 2356, FUCHS 2357, HS QUALITY, IMI 463, IMI 467, KREIDLER MS 57/2, KREIDLER MS 58A, LOGAN FORGING BRASS, MCKECHNIE W, MUNTZ PATENTS, PRYM 250, PRYM 251, PRYM 256, REVERE ALLOY NO. 380, REVERE ARCHITECTURAL BRONZE, WIELAND-Z30, WIELAND-Z31