Home » Brass Alloys » CuZn40 (C28000) Muntz Metal, Soft Material Data Sheet
CuZn40 (C28000) Muntz Metal, Soft Material Data Sheet
CuZn40 (C28000) Muntz Metal Material Data Sheet (Wrought, Soft)
CuZn40 C28000 Soft Overview
CuZn40 C28000 soft is a wrought brass (UNS C28000), known as muntz metal. Condition: Soft. This CuZn40 C28000 soft material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for CuZn40 brass parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined CuZn40 brass parts in-house and inspects them before shipment.
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
162
–
176
MPa
CuZn40 Impact & fracture properties
Fracture toughness
61.3
–
63.3
MPa.m0.5
Toughness (G)
37.2
–
40.5
kJ/m2
CuZn40 C28000 Soft Thermal properties
Melting point
882
–
902
°C
Maximum service temperature
190
–
200
°C
Minimum service temperature
-200
°C
Thermal conductivity
122
–
129
W/m.°C
Specific heat capacity
376
–
378
J/kg.°C
Thermal expansion coefficient
19.4
–
20.6
µstrain/°C
Thermal shock resistance
73.5
–
81.7
°C
Thermal distortion resistance
6.02
–
6.54
MW/m
Latent heat of fusion
220
–
240
kJ/kg
CuZn40 Electrical properties
Electrical resistivity
5.89
–
6.46
µohm.cm
Electrical conductivity
26.7
–
29.3
%IACS
Galvanic potential
-0.34
–
-0.26
V
CuZn40 Magnetic properties
Magnetic type
Non-magnetic
CuZn40 Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
3420
–
3530
m/s
Mechanical loss coefficient (tan delta)
1.56e-4
–
1.78e-4
CuZn40 Processing properties
Metal casting
Unsuitable
Metal cold forming
Limited use
Metal hot forming
Excellent
Metal press forming
Acceptable
Metal deep drawing
Limited use
Machining speed
64 m/min
Weldability Notes: Preheating and post weld heat treatments are required, and contains hazardous elements
Poor
CuZn40 Durability
Water (fresh)
Excellent
Water (salt)
Excellent
Weak acids
Acceptable
Strong acids
Unacceptable
Weak alkalis
Excellent
Strong alkalis
Excellent
Organic solvents
Excellent
Oxidation at 500C
Limited use
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Excellent
Flammability
Non-flammable
CuZn40 C28000 Soft Corrosion resistance
Stress corrosion cracking Note: Rated in ammoniacal; Other susceptible environments: Water, amine, dinitrogen tetroxide
Highly susceptible
CuZn40 Notes
CuZn40 C28000 Soft Other notes
(s)=soft; (1/2 h)=half hard; (h)=hard; (xh)=extra hard; (hr) = hot rolled; (w)=soln heat-trtd; (wh)=soln heat-trtd & work hdnd; (wp)=soln heat-trtd & precip hdnd; (whp)=precip hdnd after cold-wkng; (wph)=work hdnd after precip hdng.
CuZn40 Standards with similar compositions
Australia: 280 to AS 1567, C27400 to AS 2738, C28000 to AS 2738
Canada: HC.4.237(274) to CSA
Czech Republic: CuZn40 to CSN 423220
France: CuZn40 to NF A51-103, CuZn40 to NF A51-104
International: CuZn40 to ISO 1634, CuZn40 to ISO 1635, CuZn40 to ISO 1637, CuZn40 to ISO 1639, CuZn40 to ISO 426-1
Japan: C2800 BD to JIS H3250, C2800 BE to JIS H3250, C2800 T to JIS H3300, C2800 W to JIS H3260, C2801 P/R to JIS H3100, CuZn40 to JIS H3401
UK: CZ109 to BS 2872, CZ109 to BS 2874
USA: 60Cu-40Zn to QQ B-613, 60Cu-40Zn to QQ B-626, C27400, C27400 to ASTM B134, C27400 to ASTM B135M, C28000, C28000 to ASTM B111M, C28000 to ASTM B135M, C28000 to ASTM B36/B36M, UNS C27400, UNS C28000
Tradenames: BRASS, PIN WIRE, CERRO CF22, DELTA CF22 GENERAL PURPOSE ROD AND BAR, DELTA CF23 GENERAL PURPOSE ROD AND BAR, DELTA CF23 HIGH SPEED MACHINING ROD, FUCHS 2160, IMI 239, IMI 443, IMI 452 (MUNTZ METAL), IMI 453, MCKECHNIE SS SPECIAL, MUNTZ METAL, MUNTZ METAL NO. 3, PLUMRITE, PRYM 237, PRYM 265, REVERE ALLOY NO. 280C, SCOVILL ALLOY 280 MUNTZ METAL, SEAMLESS TUBING ALLOY, SVENSKA SM-1160, TITAN MUNTZ METAL, WIELAND-Z20, WIELAND-Z22